Embodiment 1
[0011] Example 1 Put 12g cottonseed oil, 12g soybean oil, 8g rosin, 20g rice bran oil, and 28g palm oil into a 500ml flask, start heating and stirring to fully dissolve the raw material oil in the flask, and when the temperature of the raw material oil in the flask rises to 70°C , slowly add 40g of NaOH aqueous solution with a mass concentration of 30%; control the slurry temperature in the flask to 90-100°C; react for 1 hour, add 5g of dioctyl sodium sulfosuccinate, 5g of sodium methyl palmitate, Add diethyl phthalate to the flask; continue to stir for 15 minutes to obtain a collector for phosphate rock reverse flotation to remove calcite.
[0012] Utilize the phosphate rock reverse flotation that present embodiment 1 makes to remove calcite collector to P 2 o 5 Content is 21.90%, MgO content is 0.51%, and CaO content is 51.80% Phosphorite is added 1.0kg per ton of raw ore to carry out reverse flotation to remove calcite, and obtain P 2 o 5 Concentrate of 32.48%, MgO conte...
Embodiment 2
[0013] Example 2 Take 12.75g cottonseed oil, 12.75g soybean oil, 8.5g rosin, 21.25g rice bran oil, and 29.75g palm oil and add them to a 500ml flask, start heating and stirring to fully dissolve the raw material oil in the flask; When rising to 70°C, slowly add 42g of NaOH aqueous solution with a mass concentration of 30%; control the slurry temperature in the flask to 90-100°C; react for 1 hour, add 3.75g of dioctyl sodium sulfosuccinate, 3.75g of palmitic acid Add sodium methyl sulfonate, 7.5g diethyl phthalate to the flask. Stirring was continued for 15 minutes to obtain a collector for phosphate rock reverse flotation to remove calcite.
[0014] Utilize the phosphate rock reverse flotation that embodiment 2 makes to remove calcite collector to P O content is 21.90%, and MgO content is 0.51%, and CaO content is 51.80% phosphate rock to add 1.0kg by every ton of raw ore and carry out reverse flotation Calcite was removed to obtain a concentrate with a P2O5 content of 31.78%...
Embodiment 3
[0015] Example 3 Take 13.5g cottonseed oil, 13.5g soybean oil, 9g rosin, 22.5g rice bran oil, and 31.5g palm oil and add them to a 500ml flask, start heating and stirring to fully dissolve the raw material oil in the flask, and wait until the temperature of the raw material oil in the flask rises. At 70°C, slowly add 44g of NaOH aqueous solution with a mass concentration of 30%; control the temperature of the slurry in the flask to 90-100°C, react for 1 hour, add 2.5g of dioctyl sodium sulfosuccinate, 2.5g of methyl palmitate Add sodium ester sulfonate and 5g diethyl phthalate to the flask; continue to stir for 15 minutes to obtain a collector for phosphate rock reverse flotation to remove calcite.
[0016] Utilize the phosphate rock reverse flotation that embodiment 3 makes to remove calcite collector to P O Content is 21.90%, MgO content is 0.51%, and CaO content is 51.80% Phosphorite to add 1.0kg per ton of raw ore and carry out reverse flotation Calcite was removed to obta...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com