Polypropylene high-effect photo-diffusing master batch and preparation method thereof
A light-diffusing masterbatch and high-efficiency technology, which is applied in the field of polypropylene high-efficiency light-diffusing masterbatch and its preparation, can solve the problems of PP material performance degradation, low mechanical properties of polypropylene, uneven light transmission, etc., to prevent oxidation , Improve the light transmittance, the effect of uniform light transmission distribution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] A kind of polypropylene high-efficiency light diffusion masterbatch, the raw material is weighed according to the following mass fraction:
[0028] Homopolypropylene 10: melt flow rate is 2g / 10min;
[0029] Light diffusing agent: polyorganosiloxane crosslinked microbeads 5, crosslinked (meth)acrylic polymer microbeads 5;
[0030] Transparency modifier: sorbitol derivative 1;
[0031] Dispersant: polyethylene wax 2, ester wax 2;
[0032] Lubricant: Erucamide 1;
[0033] Antioxidant 0.1.
[0034] Put the above components into a high-speed mixer, mix at 1000r / min, 110°C for 2~5min at a high speed, then extrude and knead through a twin-screw extruder at 100°C, 270r / min, cool the strands, and then Cutting, drying and sieving to get the finished product.
Embodiment 2
[0036] A kind of polypropylene high-efficiency light diffusion masterbatch, the raw material is weighed according to the following mass fraction:
[0037] Homopolypropylene 40: melt flow rate is 5g / 10min;
[0038] Light diffusing agent: polystyrene cross-linked microbeads 10, insulating glass microbeads 20;
[0039] Transparency modifier: rosin derivatives 3;
[0040] Dispersant: polyethylene wax 2, ester wax 2;
[0041] Lubricants: Polypropylene Wax 2; Zinc Stearate 2;
[0042] Antioxidant 0.5.
[0043] Put the above components into a high-speed mixer, mix at 800r / min, 115°C for 2~5min at a high speed, then extrude and knead through a twin-screw extruder at 115°C, 280r / min, cool the strands, and then Cutting, drying and sieving to get the finished product.
Embodiment 3
[0045] A kind of polypropylene high-efficiency light diffusion masterbatch, the raw material is weighed according to the following mass fraction:
[0046] Homopolypropylene 20: melt flow rate is 3g / 10min;
[0047] Light diffusing agent: cross-linked (meth)acrylic polymer microbeads 20, subnanometer barium sulfate microspheres 20;
[0048] Transparency modifier: phosphate derivatives 1, rosin derivatives 2;
[0049] Dispersant: EVA wax 2, polypropylene 4;
[0050] Lubricant: Erucamide 3;
[0051] Antioxidant 0.3.
[0052] Put the above components into a high-speed mixer, mix at a high speed of 1200r / min at 110°C for 2~5min, then extrude and knead through a twin-screw extruder at a speed of 110°C at 270r / min, cool the strands, and then Cutting, drying and sieving to get the finished product.
PUM
Property | Measurement | Unit |
---|---|---|
tensile strength | aaaaa | aaaaa |
melt flow index | aaaaa | aaaaa |
melt flow index | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com