Method for preparing wood adhesive using cassava starch hydrolyzed sugar
A technology of wood adhesive and tapioca starch, applied in the direction of adhesives, adhesive types, aldehyde/ketone condensation polymer adhesives, etc., can solve problems such as few reports on research
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] raw material
[0023] The raw materials include: the molar ratio of formaldehyde to urea F / U=1.1, the addition of melamine accounts for 3.6% of the total adhesive, and the addition of tapioca starch hydrolyzed sugar accounts for 25.5% of the total adhesive.
[0024] Wherein, tapioca starch hydrolyzed sugar is prepared according to the following operations:
[0025] 600 kg of water, 8 kg of 30% hydrochloric acid, and 300 kg of cassava starch were fed and stirred in a reaction kettle in a weight ratio of 150:2:75, and the temperature was raised to 67-72°C. The starch began to gelatinize, and then the hydrolysis reaction occurred. ;
[0026] Heat up to 89-91°C, hydrolyze until the viscosity reaches 40-45s (apply -4 cups, 30°C), cool down to 40°C, adjust pH=7.0 with 30% sodium hydroxide solution, and obtain tapioca starch hydrolyzed sugar .
[0027] method
[0028] Add 356.8 kg of 37% formaldehyde aqueous solution to the reaction kettle, adjust the pH to 4.0-4.5 with ...
Embodiment 2
[0035] raw material
[0036] The raw materials include: the molar ratio of formaldehyde to urea is F / U=1.3, the amount of melamine added accounts for 3.6% of the total amount of the adhesive, and the amount of tapioca starch hydrolyzed sugar accounts for 25.5% of the total amount of the adhesive.
[0037] Wherein, tapioca starch hydrolyzed sugar is prepared according to the following operations:
[0038] 600 kg of water, 8 kg of 30% hydrochloric acid, and 300 kg of cassava starch were fed and stirred in a reaction kettle in a weight ratio of 150:2:75, and the temperature was raised to 67-72°C. The starch began to gelatinize, and then the hydrolysis reaction occurred. ;
[0039]Heat up to 89-91°C, hydrolyze until the viscosity reaches 40-45s (apply -4 cups, 30°C), cool down to 40°C, adjust pH=7.0 with 30% sodium hydroxide solution, and obtain tapioca starch hydrolyzed sugar .
[0040] method
[0041] Add 421.6 kg of 37% formaldehyde solution in the reaction kettle, adjust...
Embodiment 3
[0049] raw material
[0050] The raw materials include: the molar ratio of formaldehyde to urea F / U=1.5, the addition of melamine accounts for 3.6% of the total adhesive, and the addition of tapioca starch hydrolyzed sugar accounts for 25.5% of the total adhesive.
[0051] Wherein, tapioca starch hydrolyzed sugar is prepared according to the following operations:
[0052] 600 kg of water, 8 kg of 30% hydrochloric acid, and 300 kg of cassava starch were fed and stirred in a reaction kettle in a weight ratio of 150:2:75, and the temperature was raised to 67-72°C. The starch began to gelatinize, and then the hydrolysis reaction occurred. ;
[0053] Heat up to 89-91°C, hydrolyze until the viscosity reaches 40-45s (apply -4 cups, 30°C), cool down to 40°C, adjust pH=7.0 with 30% sodium hydroxide solution, and obtain tapioca starch hydrolyzed sugar .
[0054] method
[0055] Add 486.5 kg of 37% formaldehyde solution in the reaction kettle, adjust the pH to 4.0-4.5 with 30% form...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com