Method for treating alkaline gold-extraction tailings by utilizing acid making tail gas
A technology for making acid tail gas and tailings, which is applied in the direction of chemical instruments and methods, non-metallic elements, and improvement of process efficiency. The effect of simple process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] A method for treating alkaline gold extraction tailings by using tail gas from acid production, comprising the following steps:
[0029] 1) Analyzing the content of sulfur, arsenic, carbon and other elements in the minerals, configuring gold concentrate containing 15% sulfur, 5% arsenic, and 1% carbon, and then adding water to stir until uniform to obtain a slurry with a concentration of 60% ; (The pulp with a concentration of 60% means that the amount of solid minerals contained in every 100 grams of pulp is 60 grams);
[0030] 2) Spray the 60% ore slurry obtained in step 1) into the roasting furnace, and roast it at a high temperature of 600°C to obtain roasting flue gas and roasted sand. The roasting flue gas is discharged from the roasting furnace Then it enters the first-level cooling dust collector and the second-level cooling dust collector in turn. The roasting flue gas in the first-level cooling dust collector and the dust-laden flue gas in the second-level coo...
Embodiment 2
[0037] A method for treating alkaline gold extraction tailings by using tail gas from acid production, comprising the following steps:
[0038] 1) Analyzing the content of elements such as sulfur, arsenic and carbon in the minerals, configuring gold concentrate containing 25% sulfur, 1% arsenic, and 1% carbon, and then adding water to stir until uniform to obtain a slurry with a concentration of 65% ; (The pulp with a concentration of 65% means that the amount of solid minerals contained in 100 grams of pulp is 65 grams);
[0039] 2) Spray the 65% ore slurry obtained in step 1) into the roasting furnace, and roast it at a high temperature of 650°C to obtain roasting flue gas and calcined sand after roasting. The roasting flue gas is discharged from the roasting furnace Then it enters the first-level cooling dust collector and the second-level cooling dust collector in turn. The roasting flue gas in the first-level cooling dust collector and the dust-laden flue gas in the secon...
Embodiment 3
[0046] A method for treating alkaline gold extraction tailings by using tail gas from acid production, comprising the following steps:
[0047] 1) Configure gold concentrate containing 20% sulfur, 10% arsenic, and 5% carbon, then add water and stir until uniform, and obtain a pulp with a concentration of 70%; (the pulp with a concentration of 70% refers to every 100 grams The amount of solid minerals contained in the pulp is 70 grams);
[0048] 2) Spray the 70% ore slurry obtained in step 1) into the roasting furnace, and roast it at a high temperature of 700°C to obtain roasting flue gas and calcined sand after roasting. The roasting flue gas is discharged from the roasting furnace Then it enters the first-level cooling dust collector and the second-level cooling dust collector in turn. The roasting flue gas in the first-level cooling dust collector and the dust-laden flue gas in the second-level cooling dust collector pass through a flue gas When the cooling device is rap...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com