A kind of la3+, al3+, fe3+, f- co-doped composite lithium-rich cathode material and preparation method thereof
A lithium-rich positive electrode material, co-doping technology, applied in the direction of battery electrodes, electrical components, circuits, etc., can solve the problems of incomplete understanding of the mechanism of action, to achieve the expansion of intercalation and deintercalation channels, good cycle capacity retention, and high ion density. The effect of conductivity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0012] Example 1: LiNO 3 :Mn(CH 3 COO) 2 4H 2 O:Ni(CH 3 COO) 2 4H 2 O:La(NO 3 ) 3 ·6H 2 O:Fe(NO 3 ) 3 9H 2 O:Al(NO 3 ) 3 9H 2 O: LiF is 1.082: 0.5365: 0.4365: 0.009: 0.009: 0.009: 0.009 (molar ratio) ratio is evenly mixed, joins in deionized water, the amount of substance added is the tartaric acid that the total amount of all metal ions is 1.2 times fully stirs to Dissolve completely; raise the temperature of the system to 70°C and continue to stir until 71% of the water evaporates, at this time the solution gradually becomes viscous and forms a jelly. The jelly-like substance was dried in an oven at 130° C. for 22 hours and then ground in a mortar for 10 minutes. The obtained powder was heated to 500°C at a rate of 2°C / min in a tube furnace and calcined at this temperature for 3 hours,
[0013] After cooling, take out the powder, continue to grind it in the mortar for 10 minutes, press the powder into a tablet with a pressure of 100 MPa, then heat up to 850°C...
Embodiment 2
[0014] Example 2: LiNO 3 :Mn(CH 3 COO) 2 4H 2 O:Ni(CH 3 COO) 2 4H 2 O:La(NO 3 ) 3 ·6H 2 O:Fe(NO 3 ) 3 9H 2 O:Al(NO 3 ) 3 9H 2 O: LiF is 1.44: 0.7125: 0.2125: 0.025: 0.025: 0.025: 0.03 (molar ratio) ratio is evenly mixed, joins in deionized water, the amount of substance added is the tartaric acid that the amount of all metal ions is 1.8 times fully stirs to Dissolve completely; raise the temperature of the system to 85°C and continue to stir until 85% of the water evaporates, then the solution gradually becomes viscous and forms a jelly. The jelly-like mass was dried in an oven at 200° C. for 48 hours and then ground in a mortar for 30 minutes. The obtained powder was heated up to 600°C at a rate of 10°C / min in a tube furnace and calcined at this temperature for 5 hours. After cooling, the powder was taken out and continued to grind in a mortar for 30 minutes, and the powder was pressed with a pressure of 300MPa. It was formed into a sheet, and then calcined in...
Embodiment 3
[0015] Embodiment 3: LiNO 3 :Mn(CH 3 COO) 2 4H 2 O:Ni(CH 3 COO) 2 4H 2 O:La(NO 3 ) 3 ·6H 2 O:Fe(NO 3 ) 3 9H 2 O:Al(NO 3 ) 3 9H 2 O: LiF is 1.152: 0.576: 0.376: 0.016: 0.016: 0.016: 0.024 (molar ratio) ratio is evenly mixed, joins in deionized water, the amount of substance added is the tartaric acid that the amount of all metal ions is 1.6 times fully stirs to Dissolve completely; raise the temperature of the system to 78°C and continue to stir until 78% of the water evaporates, at this time the solution gradually becomes viscous and forms a jelly. The jelly-like mass was dried in an oven at 170° C. for 35 hours and then ground in a mortar for 20 minutes. The obtained powder was heated up to 550°C at a rate of 7°C / min in a tube furnace and calcined at this temperature for 4 hours. After cooling, the powder was taken out and continued to grind in a mortar for 20 minutes, and the powder was pressed with a pressure of 200MPa. After being formed into a sheet, the t...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com