Stainless steel waste residue composite adsorbent and preparation method thereof
A composite adsorption, stainless steel technology, applied in chemical instruments and methods, other chemical processes, etc., can solve the problems of secondary pollution of products, small processing capacity, incomplete detoxification, etc., and achieve the effect of eliminating hidden dangers of pollution and improving utilization rate.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0012] Embodiment 1: The stainless steel waste slag composite adsorbent adopts the following raw materials and preparation methods.
[0013] Raw material weight: 1000g of cement, 5000g of stainless steel waste, 500g of 0.5mm-1.0mm sawdust and 1000g of water.
[0014] Preparation method: (1) First add water to the mixing equipment, then add cement, sawdust, and stainless steel waste slag in turn under stirring, and stir thoroughly;
[0015] (2) Extrude the uniformly stirred mixture into strips with a catalyst forming machine, and dry in an oven at 50°C to obtain the stainless steel waste slag composite adsorbent.
Embodiment 2
[0016] Embodiment 2: The stainless steel waste slag composite adsorbent uses the following raw materials and preparation methods.
[0017] Raw material weight: 2000g of cement, 6000g of stainless steel waste residue, 100g of 0.5mm-1.0mm sawdust, and 2000g of water.
[0018] Preparation method: (1) First add water to the mixing device, then add cement, sawdust, and stainless steel waste slag in turn under stirring, and stir thoroughly;
[0019] (2) Extrude the uniformly stirred mixture into strips with a catalyst molding machine, and dry in an oven at 30°C to obtain the stainless steel waste slag composite adsorbent.
Embodiment 3
[0020] Embodiment 3: The stainless steel waste slag composite adsorbent uses the following raw materials and preparation methods.
[0021] Raw material weight: cement 3500g, stainless steel waste residue 7000g, 0.5mm~1.0mm sawdust 1500g, water 3500g.
[0022] Preparation method: (1) First add water to the stirring device, then add cement, sawdust, and stainless steel waste in turn under stirring, and stir thoroughly;
[0023] (2) Extrude the uniformly stirred mixture into strips with a catalyst forming machine, and dry in an oven at 60°C to obtain the stainless steel waste slag composite adsorbent.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com