PDMS/PEI (Polydimethylsiloxane/Polyetherimide) separating membrane and preparation and application thereof
A technology for separating membranes and mass fractions, which is applied in the field of membrane materials and can solve problems such as increasing costs, reducing service life, and membrane damage
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0068] A. Preparation of Silicone Emulsion
[0069] Fully dissolve 277.2g of dodecylbenzenesulfonic acid with 2557.8g of water, weigh 3465g of D4, and add it into the mixed solution of dodecylbenzenesulfonic acid solution and keep stirring.
[0070] The mixed solution needs to be filtered through a 120-mesh filter. Use a homogenizer to homogenize and emulsify the mixed solution for 2-3 times. It must be ensured that the mixed solution entering the homogenizer is uniform, and it needs to be stirred continuously before entering the homogenizer. Silicone emulsion is milky white with bluish appearance.
[0071] The emulsion is placed in a sealed container and stored at room temperature for 2 weeks.
[0072] Detection method: take about 50ml sample and place it in a glass beaker, and observe visually from the side and the bottom under natural light. Indicators: milky white with bluish emulsion, no mechanical impurities. The viscosity of the emulsion was measured by a viscometer ...
Embodiment 2
[0083] A. Preparation of Silicone Emulsion
[0084] Fully dissolve 120.9 g of octadecyltrimethylammonium bromide with 3155.1 g of water, weigh 3024 g of D4, add it into the octadecyltrimethylammonium bromide solution and keep stirring.
[0085] The mixed liquid needs to be filtered through a 100-mesh filter. Use a homogenizer to homogenize and emulsify the mixed liquid for 2-3 times. It must be ensured that the mixed liquid entering the homogenizer is uniform, and it needs to be stirred continuously before entering the homogenizer. Silicone emulsion is milky white with bluish appearance.
[0086] The emulsion is placed in a sealed container and stored at room temperature for 3 weeks.
[0087] Detection method: take about 50ml sample and place it in a glass beaker, and observe visually from the side and the bottom under natural light. Indicators: milky white with bluish emulsion, no mechanical impurities. It was determined that the molecular weight of the silicone emulsion w...
Embodiment 3
[0097] A. Preparation of Silicone Emulsion
[0098] Fully dissolve 103.6g TX-10 with 2920.4g water, weigh 3276g D4, add it into the TX-10 solution and keep stirring.
[0099] The mixed liquid needs to be filtered through a 100-mesh filter. Use a homogenizer to homogenize and emulsify the mixed liquid for 2-3 times. It must be ensured that the mixed liquid entering the homogenizer is uniform, and it needs to be stirred continuously before entering the homogenizer. Silicone emulsion is milky white with bluish appearance.
[0100] The emulsion is placed in a sealed container and stored at room temperature for 6 weeks.
[0101] Detection method: take about 50ml sample and place it in a glass beaker, and observe visually from the side and the bottom under natural light. Indicators: milky white with bluish emulsion, no mechanical impurities. It was determined that the molecular weight of the silicone emulsion was 320,000.
[0102] B. Silicone rubber
[0103] raw materi...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com