One-step forming reflective silk screen printing ink and production method thereof
A technology for printing ink and reflective screen, applied in the direction of ink, household appliances, applications, etc., can solve the problem of limited space for reflective materials, can not use screen printing, etc., to achieve the effect of easy promotion, good reflective effect, and reduced loss.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
example 1
[0020] Example 1: Prepare 100kg red reflective screen printing ink
[0021] Weigh respectively 33kg of acrylic resin with a solid content of 100%, 3kg of dibutyl ester, 2kg of 403 anti-sedimentation agent, 3kg of BTR red, 27kg of mixed organic solvent (18 kg of ethylene glycol butyl ether, 4 kg of xylene, 5 kg of butyl acetate ), aluminum powder slurry 2kg, mix and grind until the fineness is qualified, and make the viscosity not lower than 140S, then weigh 30 kg of reflective micro-beads with a fineness of 350-800 mesh, stir well to form reflective ink, and then pour Pack.
example 2
[0022] Example 2: Preparation of 100kg blue reflective screen printing ink
[0023] Weigh respectively 15kg of polyurethane resin with 100% solid content, 3kg of dibutyl ester, 3kg of 403 anti-settling agent, 4kg of GLVO blue, 32kg of mixed organic solvent (17 kg of ethylene glycol butyl ether, 10 kg of cyclohexanone, 5 kg of xylene ), aluminum powder slurry 3kg, mix and grind until the fineness is qualified, and make the viscosity not lower than 140S, then weigh 40kg of reflective microbeads, fineness 500~800 mesh, stir well to form reflective ink, and then fill it.
example 3
[0024] Example 3: Preparation of 100kg yellow reflective screen printing ink
[0025] Weigh 30kg of polyamide resin with a solid content of 100%, 4kg of anti-settling agent, 4kg of transparent iron oxide yellow, 30kg of mixed organic solvent (ethylene glycol butyl ether 1 7 kg, butyl acetate 2 kg, isopropanol 3 kg , butanol 4 kg, xylene 4 kg), aluminum powder slurry 2kg, mix and grind until the fineness is qualified, and make the viscosity not lower than 140S, then weigh 30kg of reflective microbeads, fineness 350~800 mesh, fully Stir well into reflective ink, then fill.
PUM
Property | Measurement | Unit |
---|---|---|
solid content | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com