A technology of colored clay and rubber, which is applied in the direction of decorative art and decorative structures, can solve the problems of too hard, poor temperature adaptability, and not bright colors, etc., and achieve the effect of comfortable hand feeling, good temperature adaptability and bright colors
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] Example 1. (weight ratio)
[0024] Butadiene rubber 8 parts
[0025] 12 white ointments
[0026] Calcium carbonate (preferably ground calcium carbonate) 69 parts
[0027] 7 parts white oil
[0028] 1 part naphthenic oil
[0029] 1 part polyisobutylene
[0030] 3 parts white vaseline
[0031] Titanium dioxide 3 parts
[0032] Antioxidant 264 1.5 servings
[0033] The cis-butadiene rubber and white ointment in the above-mentioned raw materials are put into a kneader in proportion to knead to uniformity under the condition of 50-250 ℃, and then other raw materials are added in proportion to further knead to uniformity, and after cooling, extrusion molding, That is, the white clay of the present invention is obtained.
[0034] White ointment: produced by Xinji Keda Chemical Auxiliary Factory, industrial grade
[0035] White oil: Changzhou New District Petrochemical Co., Ltd. 7#
[0036] Naphthenic oil: Keyuan Lubricant Factory, Pingxiang County, Hebei Province, in...
Embodiment 2
[0038] Example 2. (weight ratio)
[0039] 8 parts of styrene butadiene rubber
[0040] 12 white ointments
[0041] Calcium carbonate (preferably ground calcium carbonate) 69 parts
[0042] 7 parts white oil
[0043] 1 part naphthenic oil
[0044] Polyisobutylene 1.5 parts
[0045] 2.5 servings of white petrolatum
[0046] Lisol Red 3144 0.5 copies
[0047] Antioxidant 264 1.5 servings
[0048] The cis-butadiene rubber and white ointment in the above-mentioned raw materials are put into a kneader in proportion to knead to uniformity under the condition of 50-250 ℃, and then other raw materials are added in proportion to further knead to uniformity, and after cooling, extrusion molding, That is, the red clay of the present invention is obtained.
[0049] Lisol Red 3144: Hangzhou Tiancai Pigment Chemical Co., Ltd.
Embodiment 3
[0050] Example 3. (weight ratio)
[0051] Butadiene rubber 8 parts
[0052] 12 white ointments
[0053] Calcium carbonate (preferably ground calcium carbonate) 60 parts
[0054] 7 parts white oil
[0055] 1 part naphthenic oil
[0056] 1 part polyisobutylene
[0057] 3 parts white vaseline
[0058] Lisol Red 0.2 to 5 servings
[0059] Antioxidant 264 1.5 servings
[0060] Fragrance appropriate amount
[0061] The cis-butadiene rubber and white ointment in the above-mentioned raw materials are put into a kneader in proportion to knead to uniformity under the condition of 50-250 ℃, and then other raw materials are added in proportion to further knead to uniformity, and after cooling, extrusion molding, That is, the red scented colored mud of the present invention is obtained.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com