Blast furnace slag liquid grinding aid and preparation method thereof
A grinding aid and liquid technology, which is applied in the field of blast furnace slag liquid grinding aid and its preparation, can solve the problems of shortage and increase, and achieve the effects of easy purchasing of raw materials, improving activity index, and increasing grinding output.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0013] Embodiment 1: a kind of liquid slag grinding aid, each component ratio is as follows (mass percentage):
[0014] Diethylene glycol 20%
[0015] Sugarcane waste liquid 15%
[0016] Sorbitol 10%
[0017] Glycerin 20%
[0018] Sodium Tripolyphosphate 5%
[0019] Sodium Carbonate 5%
[0020] The balance is water.
[0021] The preparation process of this liquid slag grinding aid is as follows:
[0022] Inject hot water at 30-40°C into the reactor, add sodium tripolyphosphate and sodium carbonate and stir for 15 minutes, then add sugar cane residue waste liquid and stir for 10 minutes; filter the materials in the reactor with a 150-mesh screen; Add diethylene glycol, sorbitol and glycerin and stir for 20 minutes to obtain a grinding aid product.
Embodiment 2
[0023] Embodiment 2: a kind of slag grinding aid, each component ratio is as follows (mass percentage):
[0024] Diethylene glycol 20%
[0025] Sugarcane waste liquid 10%
[0026] Sorbitol 10%
[0027] Glycerin 20%
[0028] Sodium Tripolyphosphate 1%
[0029] Sodium Carbonate 10%
[0030] The balance is water.
[0031] Its preparation process is with embodiment 1.
Embodiment 3
[0032] Embodiment 3: a kind of liquid cement grinding aid, each component ratio is as follows (mass percentage):
[0033] Diethylene glycol 10%
[0034] Sugarcane waste liquid 10%
[0035] Sorbitol 10%
[0036] Glycerin 20%
[0037] Sodium Tripolyphosphate 5%
[0038] Sodium Carbonate 5%
[0039] Sodium dodecylbenzenesulfonate 5%
[0040] Ethylene glycol 5%
[0041] The balance is water.
[0042] The preparation method of this liquid cement grinding aid is as follows:
[0043] Inject hot water at 30-40°C into the reaction kettle, add sodium tripolyphosphate and sodium carbonate and stir for 15 minutes, then add sugar cane residue waste liquid and stir for 10 minutes, then add ethylene glycol and sodium dodecylbenzenesulfonate Stir evenly; filter the material in the reaction kettle with a 150-mesh screen; add diethylene glycol, sorbitol, and glycerin and stir for 20 minutes to obtain a grinding aid product.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology