A technology for electrolytic manganese slag and building materials, which can be applied to buildings, building components, building structures, etc., can solve problems such as ecological damage and environmental pollution, and achieve the effects of large market capacity, low price and good quality.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0035] (1) In the electrolytic manganese slag, based on 32% (weight) of electrolytic manganese slag, 3% of additives (70% of lime, 20% of gypsum, and 10% of kaolin are crushed and mixed, and the unit is weight percentage), add appropriate amount of water and fully stir, and react in the open air for 3-5 days;
[0036] (2) In the pretreated electrolytic manganese slag, add 8% cement, 26.5% broken stone, 30% stone powder, 0.5% MNC-AE1 type rosin air-entraining agent, add water and mix uniformly;
[0037] (3) Put the mixture into a standard brick mould, form it under vibration and pressure on a QT6-15 automatic brick making machine, demould, and stack the bricks;
[0038] (4) Irrigate the adobe twice a day with clean water for the first 1-7 days, and then pour the adobe once with water the next day. After 28 days of curing, the electrolytic manganese slag standard brick can be obtained.
[0039] The produced electrolytic manganese slag standard bricks are tested, and they meet t...
Embodiment 2
[0041] (1) In electrolytic manganese slag, 36% (weight) of electrolytic manganese slag is mixed with 2% additives (75% lime, 20% gypsum, 5% kaolin and mixed after pulverization, the unit is the weight percentage), add appropriate amount of water and fully stir, and react in the open air for 4-6 days;
[0042] (2) In the electrolytic manganese slag after pretreatment, add 9% cement, 26% pebbles, 27% stone powder, add water and mix evenly;
[0043] (3) Put the mixture into a standard brick mould, form it under vibration and pressure on a QT6-15 automatic brick making machine, demould, and stack the bricks;
[0044](4) In the first 1-5 days, pour the adobe twice with clean water every day, and then pour the adobe once with water the next day. After 14 days of curing, the electrolytic manganese slag standard brick can be obtained.
[0045] The produced electrolytic manganese slag standard bricks are tested, and they meet the index requirements of MU7.5 strength grade non-load-bea...
Embodiment 3
[0047] (1) In electrolytic manganese slag, based on 35% (weight) of electrolytic manganese slag, 4.8% of additives (75% of lime, 15% of gypsum, and 10% of kaolin are crushed and mixed, and the unit is the weight percentage), add appropriate amount of water and fully stir, and react in the open air for 5-6 days;
[0048] (2) In the pretreated electrolytic manganese slag, add 10% cement, 22% gravel, 28% stone powder, 0.2% MNC-AE1 type rosin air-entraining agent, add water and mix uniformly;
[0049] (3) Put the mixture into the porous brick mould, vibrate and press on the QT6-15 full-automatic brick making machine, demould, and stack bricks;
[0050] (4) Irrigate the adobe twice a day with clean water for the first 1-6 days, and then pour the adobe once with water the next day. After curing for 28 days, the electrolytic manganese slag porous brick can be obtained.
[0051] The produced electrolytic manganese slag porous bricks are tested, and they meet the index requirements of...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com