Method for preparing nano silver sol modified by sulfonation cup arene
A technology for sulfonating calixarene and nano-silver sol, which is applied in the fields of nanomaterial chemistry and analytical chemistry, can solve the problems of unsuitable on-site detection, high time-consuming and cost, cumbersome sample processing, etc., and achieves that the modification method is simple, easy and repeatable. The effect of good performance and easy availability of ligands
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] (1) Preparation of sulfonated calix[4]arene modified nano-silver sol
[0036] At room temperature, take 2 mL of 10 -2 mol / L silver nitrate solution, respectively added to 96mL of twice distilled water and 2 ml of 10 -2 mol / L aqueous solution of sulfonated calix[4]arene, stirred for 20 minutes. Then add 8.8 mg of sodium borohydride, and continue to stir for 5 minutes, so that the nano-silver sol modified by sulfonated calix[4]arene is prepared.
[0037] Colorimetric detection of isocarbophos in sulfonated calix[4]arene modified nano-silver sol:
[0038] 0.5mL different concentrations (10 -3 -10 -7 mol / L) of isocarbophos was added to 2 mL of sulfonated calix[4]arene-modified nano-silver sol, and mixed evenly. After 10 minutes, the color of the solution changed from yellow to red.
Embodiment 2
[0040] (1) Preparation of sulfonated calix[4]arene modified nano-silver sol
[0041] At room temperature, take 2 mL of 10 -2 mol / L silver nitrate solution, respectively added to 96mL of twice distilled water and 2 ml of 10 -2 mol / L aqueous solution of sulfonated calix[4]arene, stirred for 20 minutes. Then add 4.4 mg of sodium borohydride, and continue to stir for 5 minutes, so that the nano-silver sol modified by sulfonated calix[4]arene is prepared.
[0042] Colorimetric detection of isocarbophos in sulfonated calix[4]arene modified nano-silver sol:
[0043] 0.5mL different concentrations (10 -3 -10 -7 mol / L) of isocarbophos was added to 2 mL of sulfonated calix[4]arene-modified nano-silver sol, and mixed evenly. After 10 minutes, the color of the solution changed from yellow to red.
Embodiment 3
[0045] (1) Preparation of sulfonated calix[4]arene modified nano-silver sol
[0046] At room temperature, take 2 mL of 10 -2 mol / L silver nitrate solution, respectively added to 96mL of twice distilled water and 2 ml of 10 -2 mol / L aqueous solution of sulfonated calix[4]arene, stirred for 20 minutes. Then add 8.8 mg of sodium borohydride and continue to stir for 10 minutes, so that the nano-silver sol modified by sulfonated calix[4]arene is prepared.
[0047] Sulfonated calix[4]arene modified nano-silver sol for the detection of isocarbophos:
[0048] 0.5mL different concentrations (10 -3 -10 -7 mol / L) of isocarbophos was added to 2 mL of sulfonated calix[4]arene-modified nano-silver sol, and mixed evenly. After 10 minutes, the color of the solution changed from yellow to red.
PUM
Property | Measurement | Unit |
---|---|---|
Particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com