Low-smoke bittern-free highly fire-proof elastic polyolefin electric cable material
A polyolefin cable material, high flame retardant technology, applied in the direction of insulated cables, cables, circuits, etc., can solve the problems of substitution, high material hardness, non-compliance with environmental protection requirements, etc., and achieves low hardness, good flexibility, and flame retardant performance. Good results
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0050] Example 1: A low-smoke, halogen-free and highly flame-retardant elastic polyolefin cable material
[0051] Component
parts by weight
EVA elastomer, melt index ≤ 5g / 10min, vinyl acetate content in copolymer 40% by weight
50
POE elastomer, melt index ≤ 3g / 10min, hardness ≤ 75 Shore A
36
EMA elastomer, melt index ≤ 5g / 10min, methyl acrylate content 30% by weight in the copolymer
14
Surface Treatment Magnesium Hydroxide
60
Surface treatment nano magnesium hydroxide, average particle size 40nm
25
Peroxide crosslinking agent (or vulcanizing agent)-DCP
0.3
Phenolic antioxidant (or antioxidant)-1010 antioxidant
2
3
3
Total:
193.3
[0052] Note: Surface-treated magnesium hydroxide and surface-treated nano-magnesium hydroxide refer to coating the surface of the above flame retardant...
Embodiment 2
[0057] Example 2: A low-smoke, halogen-free and highly flame-retardant elastic polyolefin cable material
[0058] Component
parts by weight
EVA elastomer, melt index ≤ 5g / 10min, vinyl acetate content in copolymer 40% by weight
70
POE elastomer, melt index ≤ 3g / 10min, hardness ≤ 75 Shore A
25
EMA elastomer, melt index ≤ 5g / 10min, methyl acrylate content 30% by weight in the copolymer
5
Surface Treatment Magnesium Hydroxide
50
Surface treatment nano magnesium hydroxide, average particle size 40nm
30
Peroxide crosslinking agent (or vulcanizing agent)-DCP
0.3
Phenolic antioxidant (or antioxidant)-1010 antioxidant
1
2
2
Total:
185.3
[0059] 2. Preparation process
[0060] It is the same as that of Embodiment 1, and the description will not be repeated.
[0061] Pilot project...
Embodiment 3
[0062] Example 3: A low-smoke, halogen-free and highly flame-retardant elastic polyolefin cable material
[0063] Component
parts by weight
EVA elastomer, melt index ≤ 5g / 10min, vinyl acetate content in copolymer 40% by weight
60
POE elastomer, melt index ≤ 3g / 10min, hardness ≤ 75 Shore A
30
EMA elastomer, melt index ≤ 5g / 10min, methyl acrylate content 30% by weight in the copolymer
10
Surface Treatment Magnesium Hydroxide
55
Surface treatment nano magnesium hydroxide, average particle size 40nm
30
Peroxide crosslinking agent (or vulcanizing agent)-DCP
0.3
Phenolic antioxidant (or antioxidant)-1010 antioxidant
1.5
2.5
2.5
Total:
191.8
[0064] 2. Preparation process
[0065] It is the same as the first embodiment, and the description will not be repeated.
PUM
Property | Measurement | Unit |
---|---|---|
melt flow index | aaaaa | aaaaa |
melt flow index | aaaaa | aaaaa |
strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com