Foamed aluminium material
A technology of foamed aluminum and aluminum liquid, applied in the field of foamed aluminum materials, can solve the problems of increasing energy consumption, affecting quality and quantity, poor hardness of foamed aluminum materials, etc., achieving fast and uniform seepage speed, reducing preparation cost, and strong sound absorption effect Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] The filler that adopts is made up of 80% kaolin, 7% white carbon black, 9% expansive soil and 4% calcium carbonate, by weight, this filler is manufactured into spherical body with granulator, the Spheroids are allowed to air dry.
[0027] Preheat the mold and the spherical body. The preheating temperature is 550°C, which is close to the temperature to be infiltrated into the molten aluminum. 6 The liquid aluminum penetrates into the gap of the spherical body within 0.5 to 10 seconds under pa. The ratio of the spherical body to the liquid aluminum is 3:1. The liquid aluminum is made of 97% industrial pure aluminum. The spheroids are washed with an aqueous solution at ~65°C, and all the spheroids are washed out from the casting, and then the foamed aluminum material is obtained.
Embodiment 2
[0029] The filler used is composed of 85% kaolin, 5% white carbon black, 7% expansive soil and 3% calcium carbonate. By weight, the filler is made into a spheroid with a granulator, and the spheroid Let the body dry naturally.
[0030] Preheat the mold and the spherical body. The preheating temperature is 600°C, which is close to the temperature to be infiltrated into the molten aluminum. 6 The liquid aluminum infiltrates into the gap of the spherical body within 0.5-10 seconds under pa. The ratio of the spherical body to the liquid aluminum is 2.5:1. The liquid aluminum is made of 97% industrial pure aluminum. The spheroids are washed with an aqueous solution at ~65°C, and a dispersant is added. The dispersant uses 0.1% sodium polyphosphate, and all the spheroids are washed out from the casting, and then the foamed aluminum material is obtained.
Embodiment 3
[0032] The filler used is composed of 92% kaolin, 3% white carbon black, 4% expansive soil and 1% calcium carbonate. By weight, the filler is made into a spheroid with a granulator, and the spheroid The body is dried at low temperature.
[0033] Preheat the mold and the spherical body. The preheating temperature is 650°C, which is close to the temperature to be infiltrated into the molten aluminum. 6 The liquid aluminum infiltrates into the gap of the spherical body within 0.5 to 10 seconds under pa. The ratio of the spherical body to the liquid aluminum is 2.5:1. The liquid aluminum is made of 97% industrial pure aluminum. The spheroids are washed with an aqueous solution at ~65°C, and a dispersant is added. The dispersant uses 0.1% sodium polyphosphate, and all the spheroids are washed out from the casting, and then the foamed aluminum material is obtained.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com