A technology of aluminum magnesium carbonate and mixed alkali solution, applied in chemical instruments and methods, aluminum compounds, inorganic chemistry, etc., can solve the problems of short anti-acid time, influence of acid-making power, inability to achieve washing, etc., to achieve excellent performance and operation. Simple and convenient effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0033] Embodiment 1 prepares hydromagnesium carbonate with the feeding mixed alkali solution of the feeding mode that disperses and drops
[0034] The molar ratio of materials is: nAl 3+ : mMg 2+ :xOH - :yCO 3 2- =1:3:9:1.0, the pH of the reaction system is controlled to be 10-11 during the dropping process. The schematic diagram of the reaction equipment is shown in figure 1 shown.
[0035] Preparation Process:
[0036] Preparation of mixed salt solution: Dissolve 150.4kg of magnesium chloride and 70.4kg of aluminum chloride into 200kg of water, stir and dissolve to form a mixed salt solution;
[0037] Preparation of mixed alkali solution: dissolve 56.2kg of sodium carbonate and 190.8kg of sodium hydroxide into 200kg of water, stir and dissolve to form a mixed alkali solution;
[0038] The prepared mixed alkali solution is dispersed and dropped into the reactor at a speed of 0.9kg / min, and the prepared mixed salt solution is added dropwise to the reactor according to ...
Embodiment 2
[0042] Embodiment 2 prepares aluminum magnesium carbonate by feeding and mixing alkali solution in the feeding mode of dispersing and dripping
[0043] The molar ratio of materials is: nAl 3+ : mMg 2+ :xOH-:yCO 3 2- = 1: 3: 14: 1.5, the pH of the reaction system is controlled during the dropping process = 11-12. The schematic diagram of the reaction equipment is shown in figure 1 shown.
[0044] Preparation Process:
[0045] Preparation of mixed salt solution: Dissolve 117.3kg of magnesium chloride and 70.4kg of aluminum sulfate in 200kg of water together to form a mixed salt solution;
[0046] Prepare mixed alkali solution: dissolve 44.5kg sodium carbonate and 151.2kg sodium hydroxide into 200kg water together to form mixed alkali solution;
[0047] Then the mixed alkali solution is dispersed and dripped into the reactor at a speed of 2.5kg / min, and the mixed salt solution prepared is added dropwise to the reactor in a conventional (single-point drip) manner to react, ...
Embodiment 3
[0050] Embodiment 3 prepares aluminum magnesium carbonate by feeding and mixing alkali solution in the feeding mode of dispersing and dripping
[0051] The molar ratio of materials is: nAl 3+ : mMg 2+ :xOH-:yCO 3 2- =1:3:12:1.2, the pH of the reaction system is controlled to be 10-11 during the dropping process.
[0052] Preparation Process:
[0053] Preparation of mixed salt solution: dissolve 191.4kg of magnesium sulfate and 70.4kg of aluminum chloride into 200kg of water to form a mixed salt solution;
[0054] Preparation of mixed alkali solution: dissolve 67.4kg of sodium carbonate and 254.4kg of sodium hydroxide into 200kg of water together to form a mixed alkali solution;
[0055] Then the mixed alkali solution is dispersed and dripped into the reactor at a speed of 1.6kg / min, and the mixed salt solution prepared is added dropwise to the reactor in a conventional (single-point drip) manner to react, and the whole process is controlled. The pH of the addition proces...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com