Powder degreasing agent, preparation method and drying device thereof
A technology of powder degreasing agent and drying device, which is applied in the field of powder degreasing agent, and can solve the problems of large consumption of degreasing agent, low alkalinity, rising cleaning cost, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0042] A preparation method of a powder degreasing agent, which is composed of the following components by weight ratio:
[0043]
[0044]
[0045] Include the following steps:
[0046] Step 1: Divide the pure water into three parts and inject them into the stirring device respectively;
[0047]Step 2, put sodium hydroxide into the first part of pure water, put the EO / PO block polymer into the second part of pure water, put the remaining components into the third part of pure water, and stir evenly;
[0048] Step 3, when the temperature of the first part of pure water and the third part of pure water is at 35-50°C, pour the third part of mixed pure water into only the first part of mixed pure water, and stir for 20-40 minutes ;
[0049] Step 4, when the temperature of the first part of pure water and the second part of pure water is at 20-35°C, pour the mixed second part of pure water into the first mixed pure water and stir for 10-20 minutes , to prepare a liquid deg...
Embodiment 2
[0053] A preparation method of a powder degreasing agent, which is composed of the following components by weight ratio:
[0054]
[0055]
[0056] Include the following steps:
[0057] Step 1: Divide the pure water into three parts and inject them into the stirring device respectively;
[0058] Step 2, put sodium hydroxide into the first part of pure water, put the EO / PO block polymer into the second part of pure water, put the remaining components into the third part of pure water, and stir evenly;
[0059] Step 3, when the temperature of the first part of pure water and the third part of pure water is at 35-50°C, pour the third part of mixed pure water into only the first part of mixed pure water, and stir for 20-40 minutes ;
[0060] Step 4, when the temperature of the first part of pure water and the second part of pure water is at 20-35°C, pour the mixed second part of pure water into the first mixed pure water and stir for 10-20 minutes , to prepare a liquid de...
Embodiment 3
[0064] A preparation method of a powder degreasing agent, which is composed of the following components by weight ratio:
[0065]
[0066]
[0067] Include the following steps:
[0068] Step 1: Divide the pure water into three parts and inject them into the stirring device respectively;
[0069] Step 2, put sodium hydroxide into the first part of pure water, put the EO / PO block polymer into the second part of pure water, put the remaining components into the third part of pure water, and stir evenly;
[0070] Step 3, when the temperature of the first part of pure water and the third part of pure water is at 35-50°C, pour the third part of mixed pure water into only the first part of mixed pure water, and stir for 20-40 minutes ;
[0071] Step 4, when the temperature of the first part of pure water and the second part of pure water is at 20-35°C, pour the mixed second part of pure water into the first mixed pure water and stir for 10-20 minutes , to prepare a liquid de...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com