Silver guidance, recovery and beneficiation method in copper-lead-zinc sulfide ore separation process
A technology of separation process and beneficiation method, applied in solid separation, flotation, etc., can solve the problem of low silver recovery rate, achieve the effect of increasing silver recovery rate, improving the comprehensive utilization rate of silver resources, and remarkable economic benefits
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0040]The raw ore of this embodiment is taken from a certain silver-containing copper-lead-zinc polymetallic sulfide ore in Inner Mongolia. t, the mass percentage of sulfur is 6.12%. Process flow chart such as figure 1 As shown, the beneficiation steps are as follows:
[0041] S1. Raw ore is ground to -0.074mm at one time, accounting for 42%;
[0042] S2. The ore pulp after the primary grinding in step S1 is subjected to copper-lead-silver mixed flotation, calculated on the basis of 1 ton of raw ore, in the copper-lead-silver mixed flotation, sodium carbonate and zinc sulfate are combined as regulators in a mass ratio of 1:1, and the combined amount It is 2600 grams, adjust the pulp pH value to be 9, and the dosage of ammonium butyl ammonium black medicine is 40 grams; Obtain copper-lead-silver mixed concentrate and copper-lead-silver mixed flotation tailings respectively;
[0043] S3. The copper-lead-silver mixed concentrate obtained in step S2 is subjected to secondary gr...
Embodiment 2
[0049] The raw ore of this embodiment is taken from a certain silver-containing copper-lead-zinc polymetallic sulfide ore in Yunnan. t, the mass percentage of sulfur is 10.96%. Process flow chart such as figure 2 As shown, the beneficiation steps are as follows:
[0050] S1. Raw ore is ground to -0.074mm at one time, accounting for 80%;
[0051] S2. The ore pulp after the primary grinding in step S1 is subjected to copper-lead-silver mixed flotation, calculated on the basis of 1 ton of raw ore, in copper-lead-silver mixed flotation, sodium carbonate and zinc sulfate are combined as regulators in a mass ratio of 4:1, and the combined amount It is 2500 grams, adjust the pulp pH value to be 9, and the dosage of butylammonium black medicine is 50 grams; Obtain copper-lead-silver mixed concentrate and copper-lead-silver mixed flotation tailings respectively;
[0052] S3. The copper-lead-silver mixed concentrate obtained in step S2 is directly subjected to copper-silver mixed fl...
Embodiment 3
[0058] The raw ore of this embodiment is taken from a certain silver-containing copper-lead-zinc polymetallic sulfide ore in Yunnan. t, the mass percentage of sulfur is 11.25%. The beneficiation steps are as follows:
[0059] S1. Raw ore is ground to -0.074mm at one time, accounting for 70%;
[0060] S2. The ore pulp after the primary grinding in step S1 is subjected to copper-lead-silver mixed flotation, calculated on the basis of 1 ton of raw ore, in copper-lead-silver mixed flotation, sodium carbonate and zinc sulfate are combined as regulators in a mass ratio of 1:1, and the combined amount It is 3000 grams, adjust the pulp pH value to be 9, and the dosage of butylammonium black medicine is 50 grams; Obtain copper-lead-silver mixed concentrate and copper-lead-silver mixed flotation tailings respectively;
[0061] S3. The copper-lead-silver mixed concentrate obtained in step S2 is secondarily ground to -0.043mm and accounts for 75%, and then copper-silver mixed flotation ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com