Non-toxic efficient rust-proof oil
An anti-rust oil and high-efficiency technology, applied in the petroleum industry, lubricating compositions, etc., can solve the problem of insignificant effect of anti-rust oil, and achieve the effect of good anti-rust effect, no pollution to the environment, and guaranteeing the quality of workpieces.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0014] The proportion of ingredients used is: 10 parts of castor oil, 3 parts of lanolin magnesium soap, 10 parts of paraffin wax, 1 part of antioxidant, 8 parts of oil-soluble gas-phase corrosion inhibitor, 4 parts of sodium molybdate, and 10 parts of film-forming agent. 8 parts, 8 parts of lauric acid, 5 parts of nano silicon dioxide, 10 parts of sodium petroleum sulfonate, 1 part of polyacrylate, 5 parts of polyoxyethylene rosin acid.
[0015] The preparation process of the present embodiment comprises the following steps:
[0016] A. Mix castor oil, lanolin magnesium soap, paraffin wax, antioxidant, and oil-soluble gas-phase corrosion inhibitor and then add it to the mixer for low-speed mixing. The mixer speed is 500 rpm and the mixing time is 20 minutes to obtain mixture A. ;
[0017] B. Add sodium molybdate, film-forming agent, lauric acid, nano-silica, sodium petroleum sulfonate, polyacrylate, polyoxyethylene rosin acid to mixture A, add it to the reaction kettle after...
Embodiment 2
[0020] The proportion of ingredients used is: 20 parts of castor oil, 8 parts of lanolin magnesium soap, 15 parts of paraffin wax, 5 parts of antioxidant, 15 parts of oil-soluble vapor phase corrosion inhibitor, 10 parts of sodium molybdate, and 15 parts of film-forming agent 12 parts, 12 parts of lauric acid, 15 parts of nano silicon dioxide, 20 parts of sodium petroleum sulfonate, 4 parts of polyacrylate, 10 parts of polyoxyethylene rosin acid.
[0021] The preparation process of the present embodiment comprises the following steps:
[0022] A. Mix castor oil, lanolin magnesium soap, paraffin wax, antioxidant, and oil-soluble gas-phase corrosion inhibitor and then add it to the mixer for low-speed mixing. The mixer speed is 500 rpm and the mixing time is 20 minutes to obtain mixture A. ;
[0023] B. Add sodium molybdate, film-forming agent, lauric acid, nano-silica, sodium petroleum sulfonate, polyacrylate, polyoxyethylene rosin acid to mixture A, add it to the reaction ket...
Embodiment 3
[0026] The proportion of ingredients used is: 12 parts of castor oil, 4 parts of lanolin magnesium soap, 11 parts of paraffin wax, 2 parts of antioxidant, 9 parts of oil-soluble vapor phase corrosion inhibitor, 5 parts of sodium molybdate, and 11 parts of film-forming agent 9 parts, 9 parts of lauric acid, 6 parts of nano silicon dioxide, 12 parts of sodium petroleum sulfonate, 2 parts of polyacrylate, 6 parts of polyoxyethylene rosin acid.
[0027] The preparation process of the present embodiment comprises the following steps:
[0028] A. Mix castor oil, lanolin magnesium soap, paraffin wax, antioxidant, and oil-soluble gas-phase corrosion inhibitor and then add it to the mixer for low-speed mixing. The mixer speed is 500 rpm and the mixing time is 20 minutes to obtain mixture A. ;
[0029] B. Add sodium molybdate, film-forming agent, lauric acid, nano-silica, sodium petroleum sulfonate, polyacrylate, polyoxyethylene rosin acid to mixture A, add it to the reaction kettle af...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com