Light-colored asphalt cement and preparation method thereof
A kind of asphalt glue, light-colored technology, applied in the field of light-colored asphalt binder and its preparation, can solve the problems of poor high-temperature stability, insufficient low-temperature crack resistance, etc., and achieve good low-temperature ductility, high softening point, and excellent road performance Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0026] A light-colored asphalt binder, in terms of mass percentage, is made of the following raw materials:
[0027]
[0028] Wherein, the antiaging agent is composed of IrganoxB900 and o-hydroxybenzophenone in a mass ratio of 1:1; the mass content of vinyl acetate in EVA (ethylene-vinyl acetate copolymer) is 26%.
[0029] A preparation method of the above-mentioned light-colored asphalt binder, the steps are as follows:
[0030] (1) According to the above ratio, weigh a certain quality of naphthenic oil into the reaction kettle, and heat it to 150-160°C;
[0031] (2) Add a certain mass of terpene resin and C5-C9 copolymerized petroleum resin according to the predetermined composition ratio and stir fully. During the whole stirring process, control the temperature at 150°C-160°C and stir fully for 15-20min until the resin Fully soluble in naphthenic oil;
[0032] (3) Raise the temperature to 165-175°C, add linear SBS and EVA, and use high-speed shearing equipment to shear...
Embodiment 2
[0035] A light-colored asphalt binder, in terms of mass percentage, is made of the following raw materials:
[0036]
[0037] Wherein, the antiaging agent is composed of IrganoxB900 and o-hydroxybenzophenone in a mass ratio of 1:1; the mass content of vinyl acetate in EVA (ethylene-vinyl acetate copolymer) is 26%.
[0038] A preparation method of the above-mentioned light-colored asphalt binder, the steps are as follows:
[0039] (1) According to the above ratio, weigh a certain quality of naphthenic oil into the reaction kettle, and heat it to 150-160°C;
[0040] (2) Add a certain mass of terpene resin and C5-C9 copolymerized petroleum resin according to the predetermined composition ratio and stir fully. During the whole stirring process, control the temperature at 150°C-160°C and stir fully for 15-20min until the resin Fully soluble in naphthenic oil;
[0041] (3) Raise the temperature to 165-175°C, add linear SBS and EVA, and use high-speed shearing equipment to shear...
Embodiment 3
[0044] A light-colored asphalt binder, in terms of mass percentage, is made of the following raw materials:
[0045]
[0046] Wherein, the anti-aging agent is composed of IrganoxB900 and o-hydroxybenzophenone in a mass ratio of 1:1; the mass content of vinyl acetate in EVA (ethylene-vinyl acetate copolymer) is 26%.
[0047] A preparation method of the above-mentioned light-colored asphalt binder, the steps are as follows:
[0048] (1) According to the above ratio, weigh a certain quality of naphthenic oil into the reaction kettle, and heat it to 150-160°C;
[0049] (2) Add a certain mass of terpene resin and C5-C9 copolymerized petroleum resin according to the predetermined composition ratio and stir fully. During the whole stirring process, control the temperature at 150°C-160°C and stir fully for 15-20min until the resin Fully soluble in naphthenic oil;
[0050] (3) Raise the temperature to 165-175°C, add linear SBS and EVA, and use high-speed shearing equipment to shear ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com