[0028] A kind of bamboo charcoal pottery, comprises each raw material of following weight portion:
[0029] Yunnan kaolin (37% aluminum content) 32 parts by weight
[0030] Yixing Zisha soil (0.15% iron content) 20 parts by weight
[0031] Dehua high white clay 4 parts by weight
[0032] Qingdao potassium feldspar 2 parts by weight
[0033] Ruizhu activated carbon 3 parts by weight
[0034] Dehua quartz stone 10 parts by weight
[0035] 15 parts by weight of bamboo charcoal
[0036] 4 parts by weight of rutile.
[0037] Its preparation method comprises the following processing steps:
[0038] (1) Raw bamboo firing: The raw bamboo is fired in a sealed carbon kiln, and the temperature of the carbon kiln is controlled below 300°C;
[0039] (2) Raw material preparation: configuring the raw materials in the above weight parts;
[0040] (3) Ball milling: Put the materials prepared in step (2) into a ball mill, add 35% of the total amount of water to be prepared, and then add...
Embodiment 2
[0046] A kind of bamboo charcoal pottery, comprises each raw material of following weight portion:
[0047] Yunnan kaolin (37% aluminum content) 35 parts by weight
[0048] Yixing Zisha soil (0.15% iron content) 23 parts by weight
[0049] Dehua high white clay 5 parts by weight
[0050] Qingdao potassium feldspar 4 parts by weight
[0051] Ruizhu activated carbon 4 parts by weight
[0052] Dehua quartz stone 12 parts by weight
[0053] 16 parts by weight of bamboo charcoal
[0054] 5 parts by weight of rutile.
[0055] Its preparation method comprises the following processing steps:
[0056] (1) Raw bamboo firing: The raw bamboo is fired in a sealed carbon kiln, and the temperature of the carbon kiln is controlled below 300°C;
[0057] (2) Raw material preparation: configuring the raw materials in the above weight parts;
[0058] (3) Ball milling: Put the materials prepared in step (2) into a ball mill, add 35% of the total amount of water to be prepared, and then add...
Embodiment 3
[0064] A kind of bamboo charcoal pottery, comprises each raw material of following weight portion:
[0065] Yunnan kaolin (37% aluminum content) 37 parts by weight
[0066] Yixing Zisha soil (0.15% iron content) 25 parts by weight
[0067] 7 parts by weight of Dehua high white clay
[0068] Qingdao potassium feldspar 5 parts by weight
[0069] Ruizhu activated carbon 5 parts by weight
[0070] Dehua quartz stone 15 parts by weight
[0071] 18 parts by weight of bamboo charcoal
[0072] 6 parts by weight of rutile;
[0073] Its preparation method comprises the following processing steps:
[0074] (1) Raw bamboo firing: The raw bamboo is fired in a sealed carbon kiln, and the temperature of the carbon kiln is controlled below 300°C;
[0075] (2) Raw material preparation: configuring the raw materials in the above weight parts;
[0076] (3) Ball milling: Put the materials prepared in step (2) into a ball mill, add 35% of the total amount of water to be prepared, and then ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.