[0014] A kind of completely biodegradable high amylose-based film of the present embodiment is prepared according to the following steps:
[0015] (1) Adjust the high-amylose starch with water to form starch milk with a mass concentration of 13%, and then use 0.3mol / L sodium hydroxide to adjust the pH value of the starch milk to 8.5, then heat the starch milk to 90°C, and heat the starch milk at 300r / min Gelatinization at stirring speed for 20min;
[0016] (2) Blending an aqueous polyvinyl alcohol solution with a mass concentration of 7% with starch milk at a stirring speed of 100 r / min, wherein the mass ratio of polyvinyl alcohol to high amylose starch is 4:6;
[0017] (3) Add an aqueous glycerin solution with a mass concentration of 15%, and plasticize it for 20 minutes under the condition of 100°C. The quality of glycerol is 20% of the total weight of starch and polyvinyl alcohol. The pH value of the hydrochloric acid regulation system of / L is 2, drips glyoxal and cross-l...
Embodiment 2
[0020] A kind of completely biodegradable high amylose-based film of the present embodiment is prepared according to the following steps:
[0021] (1) Adjust high-amylose starch with water to form starch milk with a mass concentration of 17%, then adjust the pH value of starch milk to 9.5 with 0.5mol / L sodium hydroxide, then heat the starch milk to 110°C, and heat the starch milk at 400r / min Gelatinization at stirring speed for 40min;
[0022] (2) Blending an aqueous polyvinyl alcohol solution with a mass concentration of 9% with starch milk at a stirring speed of 140 r / min, wherein the mass ratio of polyvinyl alcohol to high amylose starch is 5:5;
[0023] (3) Then add a glycerol aqueous solution with a mass concentration of 30%, and plasticize it for 40 minutes under the condition of 105 ° C. The quality of glycerin is 20 % of the total weight of starch and polyvinyl alcohol. The hydrochloric acid of L adjusts the pH value of the system to be 5, and the glyoxal is added dro...
Embodiment 3
[0026] A kind of completely biodegradable high amylose-based film of the present embodiment is prepared according to the following steps:
[0027] (1) Adjust the high amylose starch with water to form starch milk with a mass concentration of 15%, then adjust the pH value of the starch milk to 9.0 with 0.4mol / L sodium hydroxide, then heat the starch milk to 100°C, and heat the starch milk at 350r / min Gelatinization at stirring speed for 30min;
[0028] (2) Blending an aqueous polyvinyl alcohol solution with a mass concentration of 8% with starch milk at a stirring speed of 120 r / min, wherein the mass ratio of polyvinyl alcohol to high amylose starch is 6:4;
[0029] (3) Then add an aqueous glycerin solution with a mass concentration of 22.5%, and plasticize it for 30 minutes at 102.5°C. The pH value of the hydrochloric acid regulation system of / L is 3.5, drips glyoxal cross-linking reaction 40min, and glyoxal quality is 10% of starch and polyvinyl alcohol gross weight, adds 2...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com