Method for preparing spherical nickel hydroxide by using used nickel-metal hydride batteries
A spherical nickel hydroxide and nickel metal hydride battery technology, applied in battery recycling, recycling technology, process efficiency improvement and other directions, can solve the problems of low efficiency, high cost, complicated operation, etc., achieve high efficiency, reduce recycling cost, The effect of simple process operation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A method for preparing spherical nickel hydroxide using used nickel-hydrogen batteries, proceed as follows:
[0019] (1) The battery cell obtained by breaking the shell of the used Ni-MH battery is broken into powder;
[0020] (2) Take 1kg of electric core powder and add it to 30L of mixed solution composed of sulfuric acid and oxidant hydrogen peroxide (the sulfuric acid concentration is 0.5mol / L and the hydrogen peroxide concentration is 0.8ml / g), and heat to 60~65℃ , Continue to stir for 4h to obtain the extract. The concentration of the leaching solution is: Ni12-17g / L, Co0.5-1.5g / L, Re3-6g / L, Fe0.05-0.3g / L, Zn0.1-0.5g / L, Mn0.1-0.5g / L. The PH value is about 0.8-1.0.
[0021] (3) Adjust the pH value to 1.5 with 4mol / L NaOH, maintain a constant temperature of 60°C, add excess anhydrous sodium sulfate while stirring, and the rare earth elements can be precipitated in the form of rare earth sulfates. Let it stand for solid-liquid separation to obtain a rare earth-removed ...
Embodiment 2
[0027] A method for preparing spherical nickel hydroxide using used nickel-hydrogen batteries. The operation steps are similar to those in the embodiment, except that:
[0028] 1. In step (4), according to the volume ratio of the organic phase to the aqueous phase solution of 5:1, the organic solution of the extractant with a PH value of 2.8 is added to it, wherein the extractant is a mole of naphthalenesulfonic acid and pyridine carboxylic acid ester. For a compound with a ratio of 1:5, the organic solvent used in the organic solvent of the extractant is 260 mineral spirits;
[0029] 2. In step (5), the volume ratio of the organic phase to the water phase is 3:1.
Embodiment 3
[0031] A method for preparing spherical nickel hydroxide using used nickel-hydrogen batteries, proceed as follows:
[0032] (1) The battery cell obtained by breaking the shell of the used Ni-MH battery is broken into powder;
[0033] (2) Take 1kg of electric core powder and add it to 30L of mixed solution composed of sulfuric acid and oxidant hydrogen peroxide (the sulfuric acid concentration is 0.5mol / L and the hydrogen peroxide concentration is 0.8ml / g), and heat to 60~65℃ , Continue to stir for 4h to obtain the extract. The concentration of the leaching solution is: Ni12-17g / L, Co0.5-1.5g / L, Re3-6g / L, Fe0.05-0.3g / L, Zn0.1-0.5g / L, Mn0.1-0.5g / L. The PH value is about 0.8-1.0.
[0034] (3) Adjust the PH value to 1.5 with 4mol / L NaOH, maintain a constant temperature of 50°C, add excess anhydrous sodium sulfate while stirring, and the rare earth elements can be precipitated in the form of rare earth sulfates. Let it stand for solid-liquid separation to obtain a rare earth-removed ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology