Embodiment 1
[0029] (1) Preparation of Pd nanoparticles
[0030] First prepare 2mM H 2 PdCl 4 aqueous solution, and then with PVP, H 2 After O and HCl are mixed, heat to boiling, add ethanol immediately, and reflux for 3h;
[0031] (2) SiO 2 Preparation of vector
[0032] According to stober method, using TEOS as silicon source, NH 4 OH is used as a catalyst, and it is hydrolyzed at room temperature for 1 hour under the mixed system of ethanol / water;
[0033] (3) Combine the Pd nanoparticles obtained by method (1) with the SiO obtained by method (2) 2 Mix at room temperature for 24 hours to obtain Pd / SiO 2 catalyst;
[0034] (4) Pd / SiO obtained by method (3) 2 Mix the aqueous solution with the PDDA aqueous solution, let it stand at room temperature for 30 minutes, and then centrifugally wash it with deionized water for several times; then mix it with the PSS aqueous solution at room temperature for 30 minutes, and then centrifugally wash it with deionized water and methanol for seve...
Embodiment 2
[0038] (1) Preparation of Pd nanoparticles
[0039] First prepare 2mM H 2 PdCl 4 aqueous solution, and then with PVP, H 2 After O and HCl are mixed, heat to boiling, add ethanol immediately, and reflux for 3h;
[0040] (2) SiO 2 Preparation of vector
[0041] According to stober method, using TEOS as silicon source, NH 4 OH is used as a catalyst, and it is hydrolyzed at room temperature for 1 hour under the mixed system of ethanol / water;
[0042] (3) Combine the Pd nanoparticles obtained by method (1) with the SiO obtained by method (2) 2 Mix at room temperature for 24 hours to obtain Pd / SiO 2 catalyst;
[0043] (4) The catalyst obtained in method (3) was vacuum-dried overnight at 80°C and placed in a desiccator for testing.
Embodiment 3
[0045] (1) Preparation of Pd nanoparticles
[0046] First prepare 2mM H 2 PdCl 4 aqueous solution, and then with PVP, H 2 After O and HCl are mixed, heat to boiling, add ethanol immediately, and reflux for 3h;
[0047] (2) SiO 2 Preparation of vector
[0048] According to stober method, using TEOS as silicon source, NH 4 OH is used as a catalyst, and it is hydrolyzed at room temperature for 1 hour under the mixed system of ethanol / water;
[0049] (3) Combine the Pd nanoparticles obtained by method (1) with the SiO obtained by method (2) 2 Mix at room temperature for 24 hours to obtain Pd / SiO 2 catalyst;
[0050] (4) Pd / SiO obtained by method (3) 2 Mix the aqueous solution with the PDDA aqueous solution, let it stand at room temperature for 30 minutes, and then centrifugally wash it with deionized water for several times; then mix it with the PSS aqueous solution at room temperature for 30 minutes, and then centrifugally wash it with deionized water and methanol for se...
PUM
![No PUM](https://static-eureka-patsnap-com.libproxy1.nus.edu.sg/ssr/23.2.0/_nuxt/noPUMSmall.5c5f49c7.png)
Abstract
Description
Claims
Application Information
![application no application](https://static-eureka-patsnap-com.libproxy1.nus.edu.sg/ssr/23.2.0/_nuxt/application.06fe782c.png)
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com