Sizing agent for paper
A technology of sizing agent and glue, which is applied in the direction of papermaking, paper coating, water repellent addition, etc., can solve the problems of low weight, high strength, insufficient strength indicators such as compression resistance and tearing of paper, and achieve anti-corrosion High tear strength, good smoothness, good surface printing adaptability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] Dissolve edible corn starch in water to form an aqueous starch solution with a mass fraction of 20%, add biological enzymes (industrial enzyme preparations) accounting for 0.005% of the starch mass, enzymatic treatment at 80-82 ° C for 15 minutes, and then heat to 130-135 Cook at ℃ for 0.5-1 minutes to inactivate the enzyme to obtain a glue solution, add polyvinyl alcohol with a mass of 1% of the glue solution, cationic styrene acrylate with a mass of 2% of the glue solution, and a mass of 1% of the glue solution. 2% of aluminum sulfate in the glue solution, 0.1% of the fatty acid ester in the glue solution, and 0.2% of the cationic yellow dye in the glue solution are mixed uniformly to obtain the sizing agent for paper of the present invention.
Embodiment 2
[0022] Dissolve edible corn starch in water to form a starch aqueous solution with a mass fraction of 25%, add biological enzymes (industrial enzyme preparations) accounting for 0.01% of the starch mass, enzymatic treatment at 83-85 ° C for 20 minutes, and then heat to 135-140 Cook at ℃ for 0.5-1 minute to inactivate the enzyme to obtain a glue solution, add polyvinyl alcohol with a mass of 2% of the glue solution, cationic styrene acrylate with a mass of 4% of the glue solution, and a mass of 2% of the glue solution. 4% of aluminum sulfate in the glue solution, 0.3% of the fatty acid ester in the glue solution, and 0.6% of the cationic yellow dye in the glue solution are mixed uniformly to obtain the sizing agent for paper of the present invention.
Embodiment 3
[0024] Dissolve edible corn starch in water to form a starch aqueous solution with a mass fraction of 23%, add biological enzymes (industrial enzyme preparations) accounting for 0.008% of the starch mass, enzymatic treatment at 80-85 ° C for 10 minutes, and then heat to 130-135 Cooking at ℃ for 0.5 to 1 minute to inactivate the enzyme to obtain a glue solution, add polyvinyl alcohol with a mass of 1.5% of the glue solution, cationic styrene acrylate with a mass of 3% of the glue solution, and a mass of 1.5% of the glue solution. 3% of aluminum sulfate in the glue solution, 0.2% of the fatty acid ester in the glue solution, and 0.4% of the cationic yellow dye in the glue solution are mixed uniformly to obtain the sizing agent for paper of the present invention.
[0025] After the sizing agent of the present invention prepared in the above example is used in papermaking, it can significantly improve the physical properties of the finished paper such as break resistance, ring ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com