Auxiliary door/window frame made of biomass composite materials and manufacturing method of auxiliary door/window frame
A technology of composite materials and manufacturing methods, applied in the direction of the base frame, etc., can solve the problems of short service life of the sub-frames of doors and windows, unfavorable energy saving and heat preservation of buildings, and easy decay and deterioration of wood, so as to improve energy saving and heat preservation performance, improve heat insulation performance and The effect of structural strength and low cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] 1) Select raw materials:
[0036] ①Wood flour: 40 parts, the fineness is 100 mesh, and the moisture content is 3%;
[0037] ②Calcium carbonate, talcum powder, glass fiber mixed in any proportion: 5 parts;
[0038] ③PVC: 40 copies;
[0039] 2) After fully mixing the above materials, granulate;
[0040] 3) Put the granulated material into the extruder for extrusion molding; the temperature of the extruder is 180 degrees Celsius, and the pressure is 60MPA;
[0041] 4) After the formed material is surface processed and tenon groove processed, it is made into a door and window sub-frame.
Embodiment 2
[0043] 1) Select raw materials:
[0044] ①Straw powder: 55 parts, with a fineness of 40 mesh and a moisture content of 5%;
[0045] ②Calcium carbonate, talcum powder, glass fiber mixed in any proportion: 10 parts;
[0046] ③PE: 35 copies;
[0047] 2) After fully mixing the above materials, granulate;
[0048] 3) Put the granulated material into the extruder for extrusion molding; the temperature of the extruder is 240 degrees Celsius, and the pressure is 25MPA;
[0049] 4) After the formed material is surface processed and tenon groove processed, it is made into a door and window sub-frame.
Embodiment 3
[0051] 1) Select raw materials:
[0052] ①Wood flour: 65 parts, the fineness is 120 mesh, and the moisture content is 2%;
[0053] ②Arbitrarily mixed calcium carbonate and glass fiber: 8 parts;
[0054] ③PP: 30 copies;
[0055] 2) After fully mixing the above materials, granulate;
[0056] 3) Put the granulated material into the extruder for extrusion molding; the temperature of the extruder is 200 degrees Celsius, and the pressure is 40MPA;
[0057] 4) After the formed material is surface processed and tenon groove processed, it is made into a door and window sub-frame.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com