Synthetic method of novel tackifying resin
A technology of tackifying resin and synthesis method, which is applied in the field of synthesis of new tackifying resin, can solve the problems of damp heat resistance, poor washing resistance, unsatisfactory effect, etc., and achieve good water resistance, good economic benefits and market prospects.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0012] (1) Mix tert-butylphenol, abietic acid, toluene, and sulfuric acid in proportions by weight of tert-butylphenol:abietic acid:toluene:sulfuric acid at 25:30:90:0.5, heat up to 130°C for reflux dehydration reaction for 4 hours ;
[0013] (2) After dehydration, slowly add 37% formaldehyde solution, heat to 90°C and reflux for 3.5 hours;
[0014] (3) Add 30% NaOH solution for neutralization, after washing with water, evaporate the volatile matter under the condition of negative pressure 0.05~0.08mpa, kettle temperature 200~210℃, take a sample after 30-35 minutes and measure the softening point when it reaches 125℃, put material, that is, a new type of tackifying resin.
[0015] Wherein above-mentioned steps add tert-butylphenol, abietic acid, toluene, sulfuric acid, formaldehyde solution by weight ratio tert-butylphenol:abietic acid:toluene:sulfuric acid:formaldehyde solution is 25:30:90:0.5:15.
Embodiment 2
[0017] (1) Mix tert-butylphenol, abietic acid, toluene, and sulfuric acid in proportions by weight of tert-butylphenol:abietic acid:toluene:sulfuric acid at 40:60:100:5, heat up to 160°C for reflux dehydration reaction for 5 hours ;
[0018] (2) After dehydration, slowly add 37% formaldehyde solution, heat to 90~110°C and reflux for 4 hours;
[0019] (3) Add 30% NaOH solution for neutralization, after washing with water, evaporate the volatile matter under the condition of negative pressure 0.05-0.08mpa, kettle temperature 200-210℃, take a sample after 30-35 minutes and measure the softening point when it reaches 155℃, put material, that is, a new type of tackifying resin.
[0020] Wherein in the above-mentioned step, add tert-butylphenol, abietic acid, toluene, sulfuric acid, formaldehyde solution by weight ratio tert-butylphenol: abietic acid: toluene: sulfuric acid: formaldehyde solution is 40: 60: 100: 5: 40.
Embodiment 3
[0022] (1) Mix tert-butylphenol, abietic acid, toluene, and sulfuric acid in proportions by weight of tert-butylphenol:abietic acid:toluene:sulfuric acid at 30:30:100:0.6, heat up to 140°C for reflux dehydration reaction for 4 hours , the dehydration rate reaches 77.8%;
[0023] (2) After dehydration, slowly add 37% formaldehyde solution, heat to 95°C and reflux for 3.5 hours;
[0024] (3) Add 30% NaOH solution for neutralization, after washing with water, evaporate the volatile matter under the conditions of negative pressure 0.05-0.08mpa, kettle temperature 200-210°C, take a sample after 30-35 minutes and measure the softening point when it reaches 140°C, put material, that is, a new type of tackifying resin.
[0025] Wherein above-mentioned steps add tert-butylphenol, abietic acid, toluene, sulfuric acid, formaldehyde solution in proportion by weight tert-butylphenol:abietic acid:toluene:sulfuric acid:formaldehyde solution is 30:30:100:0.6:20.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com