Method for manufacturing luminous bowling ball groove
A production method and bowling ball technology are applied in the field of the production of luminous bowling ball lanes, which can solve problems such as no reports on luminous ball lanes, and achieve the effect of reducing costs.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0038] Making fluorescent signs
[0039] a resin modulation
[0040] Prepare raw materials according to the following weight ratio: melamine resin 30%, phenolic resin 11%, water 50%, coupling agent (KH550) 1%, water-soluble fluorescent whitening agent 5%, water-soluble long-lasting luminous powder 2%, water-soluble Light stabilizer 1%; then, slowly add melamine resin, phenolic resin, coupling agent, water-soluble fluorescent whitening agent, water-soluble long-lasting luminous powder, water-soluble light stabilizer to the water in order, stir while adding, stir 25 minutes until uniform;
[0041] b Adhesive paper production
[0042] Use 18 g / m2 surface paper, impregnate the resin prepared in step a with a dipping line, dry, and cut the film paper into sheets; the glue content of the film paper is 10%, and the volatile matter is 7%.
[0043] c logo making
[0044] Cut the adhesive film in step b into an equilateral triangle with a side length of 50MM, and keep it sealed to ...
Embodiment 2
[0063] Making fluorescent signs
[0064] a resin modulation
[0065] Prepare raw materials according to the following weight ratio: melamine resin 30%, phenolic resin 11%, water 50%, coupling agent (KH550) 1%, water-soluble fluorescent whitening agent 5%, water-soluble long-lasting luminous powder 2%, water-soluble Light stabilizer 1%; then, slowly add melamine resin, phenolic resin, coupling agent, water-soluble fluorescent whitening agent, water-soluble long-lasting luminous powder, water-soluble light stabilizer to the water in order, stir while adding, stir 20 minutes until uniform;
[0066] b Adhesive paper production
[0067] Use 18 g / m2 surface paper, impregnate the resin prepared in step a with a dipping line, dry, and cut the film paper into sheets; the glue content of the film paper is 20%, and the volatile matter is 6%.
[0068] c logo making
[0069] Cut the adhesive film in step b into an equilateral triangle with a side length of 50MM, and keep it sealed to ...
Embodiment 3
[0085] Making fluorescent signs
[0086] a resin modulation
[0087] Prepare raw materials according to the following weight ratio: melamine resin 30%, phenolic resin 11%, water 50%, coupling agent (KH550) 1%, water-soluble fluorescent whitening agent 5%, water-soluble long-lasting luminous powder 2%, water-soluble Light stabilizer 1%; then, slowly add melamine resin, phenolic resin, coupling agent, water-soluble fluorescent whitening agent, water-soluble long-lasting luminous powder, water-soluble light stabilizer to the water in order, stir while adding, stir 30 minutes until uniform;
[0088] b Adhesive paper production
[0089] Use 18 g / m2 surface paper, impregnate the resin prepared in step a with a dipping line, dry, and cut the film paper into sheets; the glue content of the film paper is 15%, and the volatile matter is 6.5%.
[0090] c logo making
[0091] Cut the adhesive film in step b into an equilateral triangle with a side length of 50MM, and keep it sealed t...
PUM
Property | Measurement | Unit |
---|---|---|
Tensile strength | aaaaa | aaaaa |
Tensile strength | aaaaa | aaaaa |
Tensile strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com