Embodiment 1
[0019] Taking 100kg of water for preparing cleaning solution as an example, the method steps for cleaning porous asphalt pavement voids are as follows:
[0020] 1. Vacuum the sundries in the gaps of porous asphalt pavement
[0021] Use a vacuum cleaner to vacuum the clogged sundries in the gaps of the porous asphalt pavement for 15 to 20 seconds, and the vacuum degree of the vacuum cleaner is 21.
[0022] 2. Prepare cleaning solution
[0023] Add 4kg of QW-917 road cleaner into 100kg of water, stir evenly, form foam, and prepare cleaning solution.
[0024] 3. Rinse porous asphalt pavement with high-pressure cleaning fluid
[0025] Spray the cleaning solution with a pressure of 5MPa from a cold water high-pressure cleaner into the porous asphalt pavement after vacuuming for 20 seconds, with an interval of 10 minutes.
Embodiment 2
[0027] Taking 100kg of water for preparing cleaning solution as an example, the method steps for cleaning porous asphalt pavement voids are as follows:
[0028] In step 2 of preparing the cleaning solution, add 2 kg of QW-917 road cleaner to 100 kg of water, stir evenly, form foam, and prepare cleaning solution. In the step 3 of flushing the porous asphalt pavement with high-pressure cleaning fluid, spray the cleaning fluid with a pressure of 3MPa from a cold water high-pressure cleaner into the porous asphalt pavement after vacuuming for 15 seconds, with an interval of 10 minutes, and then use a high-pressure cleaning fluid with a pressure of 8 MPa from a cold water high-pressure cleaner Rinse the porous asphalt pavement with a 25-second flush. Other steps are identical with embodiment 1.
Embodiment 3
[0030] Taking 100kg of water for preparing cleaning solution as an example, the method steps for cleaning porous asphalt pavement voids are as follows:
[0031] In step 2 of preparing the cleaning solution, add 8 kg of QW-917 road cleaner to 100 kg of water, stir evenly, form foam, and prepare cleaning solution. In step 3 of flushing the porous asphalt pavement with high-pressure cleaning fluid, spray the cleaning fluid with a pressure of 7 MPa from a cold water high-pressure cleaner into the porous asphalt pavement after vacuuming for 25 seconds, with an interval of 10 minutes, and then use a high-pressure cleaning fluid with a pressure of 12 MPa from a cold water high-pressure cleaner Rinse the porous asphalt pavement with a 35-second flush. Other steps are identical with embodiment 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology