Method for preparing aluminium powder with high tap density
A technology of bulk density and silver powder, applied in the field of electronic materials, can solve the problems of high cost, expensive production equipment, unfavorable industrialization promotion, etc., and achieve the effect of low cost and easy operation.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0009] A preparation method of silver powder with high bulk density, 100 parts by weight of silver nitrate and 1 part by weight of nitric acid are dissolved in deionized water to form a silver nitrate solution with a concentration of 30-60%; 50-65 parts by weight of sodium carbonate Dissolve in deionized water to form a sodium carbonate solution with a concentration of 5-25%; under continuous stirring, add the above-mentioned silver nitrate solution to the sodium carbonate solution to obtain a precursor silver carbonate system, at this time The mixed solution of the mixture is weakly alkaline; control the temperature of the above precursor silver carbonate system at 15°C-25°C, and quickly add a strong reducing agent to complete the reduction reaction under continuous stirring conditions. After the reduction is completed, wash with deionized water for 15-20 After three times, deionized water was filtered out and dried to obtain the desired silver powder.
[0010] The strong red...
Embodiment 1
[0016] 1. Weigh 100 parts by weight of silver nitrate, dissolve it in 150 parts by weight of deionized water, then add 1 part by weight of nitric acid to the silver nitrate solution, fully stir and mix, and set aside;
[0017] 2. Weigh 60 parts by weight of sodium carbonate, dissolve it in 200 parts by weight of deionized water, stir well, set aside,
[0018] 3. Under the condition of continuous stirring, add the silver nitrate solution to the sodium carbonate solution to prepare the precursor silver carbonate;
[0019] 4. Weigh 10 parts by weight of hydrazine hydrate, dissolve in 10 parts by weight of deionized water, stir well and set aside;
[0020] 5. Using a water bath, adjust the temperature of the silver carbonate solution system in step 3 to 15°C, and add the hydrazine hydrate solution in step 4 to the silver carbonate solution quickly under continuous stirring to complete the reduction;
[0021] 6. Wash the reduced silver powder mixed solution with deionized water 20...
Embodiment 2
[0023] 1. Weigh 100 parts by weight of silver nitrate, dissolve it in 100 parts by weight of deionized water, then add 1 part by weight of nitric acid to the silver nitrate solution, fully stir and mix, and set aside;
[0024] 2. Weigh 60 parts by weight of sodium carbonate, dissolve it in 240 parts by weight of deionized water, stir well, set aside,
[0025] 3. Under the condition of continuous stirring, add the silver nitrate solution to the sodium carbonate solution to prepare the precursor silver carbonate;
[0026] 4. Weigh 10 parts by weight of hydrazine hydrate, dissolve in 10 parts by weight of deionized water, stir well and set aside;
[0027] 5. Using a water bath, adjust the temperature of the silver carbonate solution system in step 3 to 20°C, and under continuous stirring, quickly add the hydrazine hydrate solution in step 4 into the silver carbonate solution to complete the reduction;
[0028] 6. Wash the reduced silver powder mixed solution with deionized water...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com