Environment-friendly color-changing method of synthetic leather bass
An environmentally friendly, synthetic leather technology, applied in fiber processing, textiles and papermaking, etc., can solve the technical defects of water-based polyurethane and other problems, achieve excellent bonding fastness, improve the working environment, and save energy consumption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] (1) Preparation of water-based color-changing slurry:
[0020] Add 100kg of water-based polyurethane resin and 20kg of black water-based color paste into a container with a stirrer and stir at room temperature for 25 minutes for later use.
[0021] (2) Preparation of color-changing layer
[0022] Apply the above-mentioned color-changing slurry evenly on the synthetic leather base by roller coating method, the sizing amount is 80g / m, the drying speed is 15m / min, and the drying temperature is 80°C.
[0023] (3) Mechanical embossing
[0024] After the water in the above-mentioned color-changing layer is completely volatilized, emboss by rolling, with a rolling pressure of 25MPa, a rolling temperature of 180°C, and a rolling speed of 15m / min.
Embodiment 2
[0026] (1) Preparation of water-based color-changing slurry:
[0027] Add 200kg of water-based polyurethane resin, 60kg of brown water-based color paste, 3kg of thickener and 1kg of leveling agent into a container with a stirrer and stir at room temperature for 25 minutes for later use.
[0028] (2) Preparation of color-changing layer
[0029] Apply the above-mentioned color-changing slurry evenly on the synthetic leather base by spraying method, the sizing amount is 100g / m, the drying speed is 15m / min, and the drying temperature is 90°C.
[0030] (3) Mechanical embossing
[0031] After the water in the above-mentioned color-changing layer is completely volatilized, emboss by plate pressing, the plate pressing pressure is 15Mpa, the plate pressing temperature is 80°C, and the time is 3s.
Embodiment 3
[0033] (1) Preparation of water-based color-changing slurry:
[0034] Add 300kg of water-based polyurethane resin, 120kg of beige water-based color paste, 9kg of thickener, 3kg of leveling agent and 3kg of cross-linking agent into a container with a stirrer and stir at room temperature for 30 minutes for later use.
[0035] (2) Preparation of color-changing layer
[0036] The above-mentioned color-changing paste is evenly coated on the synthetic leather base by the three-plate printing method, the sizing amount is 120g / m, the drying speed is 20m / min, and the drying temperature is 100°C.
[0037] (3) Mechanical embossing
[0038] After the water in the above-mentioned color-changing layer is completely volatilized, embossing is carried out by plate pressing, with a plate pressure of 18Mpa, a plate temperature of 90°C, and a time of 5 seconds.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com