Method for producing sodalite pure phase with shale ash
A technology of oil shale ash and sodalite, which is applied in the field of production and preparation of inorganic functional materials, can solve the problems of difficulty in obtaining pure phase of zeolite molecular sieve, cumbersome process steps, and high production cost, and achieve simple pretreatment, simple process, and equipment less demanding effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0014] (1) Grind the oil shale ash and pass it through a 100-mesh sieve. Dry in an oven at 90°C for 24 hours.
[0015] The XRF elemental analysis results of its chemical composition are as follows:
[0016] chemical composition
SiO 2
al 2 o 3
Fe 2 o 3
CO 2
K 2 o
TiO 2
percentage%
73.8
19.3
2.2
2.2
0.8
0.6
[0017] (2) Mole ratio H 2 O / Na 2 O=5 Weigh sodium hydroxide and deionized water, mix them in a polyethylene bottle, and press NaOH 2 O / SiO 2 =3 Add oil shale ash and stir for 0.5h to mix well.
[0018] (3) The above reaction mixture was transferred to a stainless steel reaction kettle, sealed and then placed in a 180°C electric constant temperature drying oven for crystallization for 24 hours.
[0019] (4) Take out the reaction kettle, perform suction filtration after cooling, wash until pH = 7, and put it in an oven at 100° C. to dry to obtain sodalite crystal powder.
Embodiment 2
[0021] (1) Grind the oil shale ash and pass it through a 100-mesh sieve. Dry in an oven at 100°C for 24 hours.
[0022] (2) Mole ratio H 2 O / Na 2 O=7.8 Weigh sodium hydroxide and deionized water, mix them in a polyethylene bottle, and press Na 2 O / SiO 2 =7 Add oil shale ash and stir for 1 hour to mix well.
[0023] (3) The above reaction mixture was transferred to a stainless steel reaction kettle, sealed and placed in a 160°C electric constant temperature drying oven for crystallization for 70 hours.
[0024] (4) Take out the reaction kettle, perform suction filtration after cooling, wash until pH = 7, and put it in an oven at 100° C. to dry to obtain sodalite crystal powder.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com