Free oiling and self-lubricating elevator guideway guide shoes and preparation method thereof
An elevator guide rail and self-lubricating technology, which is applied in the field of elevators, can solve problems such as dirty elevator rails and bridge compartments, shortened service life, and high operating noise, and achieves simple and easy preparation methods, long service life, and small friction coefficient Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] The weight percent of each component in the raw material formula is as follows:
[0020] PTFE 75%
[0021] Carbon Fiber 18%
[0023] The steps of the manufacturing process are as follows: (1) preparing raw materials according to the formula; (2) placing the prepared raw materials on tooling molds; (3) die-casting; (4) testing surface hardness and smoothness; (5) vacuum insulation.
[0024] The die-casting process adopts 100kg / cm 2 Pressure compression molding.
[0025] The temperature of the vacuum insulation is 100° C., and the insulation time is 20 hours.
Embodiment 2
[0027] The weight percent of each component in the raw material formula is as follows:
[0028] PTFE 85%
[0029] Carbon Fiber 12%
[0031] The steps of the manufacturing process are as follows: (1) preparing raw materials according to the formula; (2) placing the prepared raw materials on tooling molds; (3) die-casting; (4) testing surface hardness and smoothness; (5) vacuum insulation.
[0032] The die-casting process adopts 300kg / cm 2 Pressure compression molding.
[0033] The temperature of the vacuum insulation is 400° C., and the insulation time is 12 hours.
Embodiment 3
[0035] The weight percent of each component in the raw material formula is as follows:
[0036] PTFE 80%
[0037] Carbon Fiber 15%
[0038] Bronze powder 5%.
[0039] The steps of the manufacturing process are as follows: (1) preparing raw materials according to the formula; (2) placing the prepared raw materials on tooling molds; (3) die-casting; (4) testing surface hardness and smoothness; (5) vacuum insulation.
[0040] The die casting forming process adopts 200kg / cm 2 Pressure compression molding.
[0041] The temperature of the vacuum heat preservation is 200° C. to 300° C., and the heat preservation time is 15 to 18 hours.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com