Sludge petroleum charred slurry and preparing process and application thereof
A technology of petroleum coke and sludge, which is applied in the petroleum industry, coke ovens, special forms of dry distillation, etc., can solve the problems of inability to provide heat and heat loss, achieve large-scale industrial application prospects, improve pulping performance, and reduce secondary pollution Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] 1. Raw material
[0030] (1) Sewage sludge produced by a sewage treatment plant, water content ------80% (weight);
[0031] (2) Petroleum coke from a refinery, sulfur content ------ 0.6%, ash content ------ 0.8%;
[0032] (3) Dispersant (sodium lignosulfonate);
[0033] (4) Sludge modification agent (sodium carbonate);
[0034] (5) water.
[0035] 2. Preparation conditions
[0036] (1) Raw material ratio (parts by weight)
[0037] 100 parts of petroleum coke, 25 parts of hydrous sludge, 50 parts of water, 0.01 part of dispersant, and 0.01 part of sludge modifier.
[0038] (2) Preparation method
[0039] Firstly, the sewage sludge is fully mixed with the sludge modifying agent, and left for 4 hours to obtain the modified sludge. Then grind and mix the modified sludge, petroleum coke, water and dispersant to make high-concentration sludge petroleum coke slurry.
[0040] 3. Product performance indicators
[0041] (1) Appearance shape --- gray black paste. At 25°C...
Embodiment 2
[0048] 1. Raw materials
[0049] (1) Sewage sludge produced by a sewage treatment plant, water content ------80% (weight);
[0050] (2) Petroleum coke from a refinery, sulfur content ------ 4%, ash content ------ 0.6%;
[0051] (3) Dispersant (sodium methylnaphthalenesulfonate formaldehyde condensate);
[0052] (4) Sludge modification agent (calcium hydroxide);
[0053] (5) water.
[0054] 2. Preparation conditions
[0055] (1) Raw material ratio (parts by weight)
[0056] 150 parts of petroleum coke, 45 parts of sewage sludge, 60 parts of water, 1 part of dispersant, 0.5 parts of sludge modifier.
[0057] (2) Preparation method
[0058] First, the sewage sludge is fully mixed with the sludge modifying agent, and left for 3 days to obtain the modified sludge. Then grind and mix the modified sludge, petroleum coke, water and dispersant to make high-concentration sludge petroleum coke slurry.
[0059] 3. Product performance indicators
[0060] (1) Appearance shape --- g...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
shear viscosity | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com