Method for ash-free and no-sulfurizing alkaline liming treatment for making pigskin leather
A technology of alkali sulfide and pigskin, applied in chemical treatment of small raw hide/large raw hide/leather hide/fur, small raw hide/large raw hide/leather/fur treatment, chemical treatment before tanning, etc., can solve the problem of excessive elongation , loose surface, tube wrinkle and other problems
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] Embodiment 1: pigskin suede garment leather technology
[0031] (1) Immersion
[0032] The raw hides are weighed and washed with water, and the water is controlled. Take 100 kg of rawhide and put it into the drum, add 150 kg of water at 20°C, 2 kg of ammonium bicarbonate into the drum, rotate for 30 minutes, adjust the pH of the solution to 8.0, then add 0.6 kg of anionic degreasing agent and mixed enzyme 0.5 kg, rotate for 120 minutes, stop soaking for 12 hours, drain, add 3 kg of salt, 0.2 kg of preservative, rotate for 20 minutes, and let out the drum.
[0033] (2) Enzyme hair removal
[0034] Take 100 kg of rawhide, 0.2 kg of mixed enzyme, 0.5 kg of 1398 protease, 7 kg of sawdust, 10 kg of water, mix thoroughly, brush on the back of the buttocks with a brush, stack for 42 hours, keep the pH value at 7.8, and push the hair by machine.
[0035] (3) Expansion
[0036] Take 100 kg of fur and put it into the drum, add 120 kg of water at a temperature of 20 °C, 1.5 kg...
Embodiment 2
[0041] Embodiment 2: pigskin upper leather technology
[0042] (1) Immersion
[0043] The raw hides are weighed and washed with water, and the water is controlled. Take 100 kg of raw hide and put it into the drum, add 150 kg of water at 22 ° C, 2.5 kg of ammonium bicarbonate into the drum, rotate for 25 minutes, adjust the pH of the solution to 7.8, then add 0.4 kg of anionic degreasing agent and mixed enzyme 0.3 dry grams, rotate for 150 minutes, stop soaking for 10 hours, drain, add 5 kg of salt, 0.3 kg of preservatives, rotate for 30 minutes, and let out the drum.
[0044] (2) Enzyme hair removal
[0045] Take 100 kg of raw hide, 0.4 kg of mixed enzyme, 0.3 kg of 1398 protease, 6 kg of sawdust, 12 kg of water, mix thoroughly, brush on the back of the buttocks with a brush, pile up for 36 hours, keep the pH value at 8.5, and push the hair by machine.
[0046] (3) Expansion
[0047] Weigh the push fur, take 100 kg, put it into the drum, add 100 kg of water with a temperat...
Embodiment 3
[0052] Embodiment 3: Pigskin front garment leather technology
[0053] (1) Immersion
[0054] The raw hides are weighed and washed with water, and the water is controlled. Take 100 kg of rawhide and put it into the drum, add 150 kg of water with a temperature of 18 ℃, 3 kg of ammonium bicarbonate into the drum, rotate for 20 minutes, adjust the pH value of the solution to 8.5, then add 0.3 kg of anionic degreasing agent and mixed enzyme 0.4 kg, rotate for 130 minutes, stop soaking for 11 hours, drain, add 4 kg of salt, 0.4 kg of preservative, rotate for 25 minutes, and let the drum out.
[0055] (2) Enzyme hair removal
[0056] Take 100 kg of raw hide, 0.3 kg of mixed enzyme, 0.4 kg of 1398 protease, 5 kg of sawdust, 15 kg of water, mix thoroughly, brush on the back of the buttocks with a brush, pile up for 40 hours, keep the pH value at 8.0, and push the hair by machine.
[0057] (3) Expansion
[0058] Weigh the push fur, take 100 kg, put it into the drum, add 150 kg of w...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com