A light-colored cementing material and road-use technology, applied in the direction of roads, roads, adhesives, etc., can solve the problems that colored asphalt cannot completely get rid of dark brown, cannot be uniformly dispersed in three components, and the color effect is not good, so as to achieve beautification and decoration Effects of living environment and sports facilities, simple construction, easy organization and control of transportation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] A preparation method of light-colored cement for roads comprises the following steps and process conditions:
[0021] Step 1: Preparation of polymer matrix
[0022] (A) Proportion of polymer matrix
[0023] Based on 100 parts by mass of polymer, 100 parts by mass of styrene-butadiene-styrene triblock thermoplastic elastomer SBS and 400 parts by mass of naphthenic oil filled with rubber;
[0024] (B) According to the ratio of (A), put each component into a high-shear force open-type rubber mixer for blending. The mixing temperature is 80°C, and the mixing time is 30 minutes.
[0025] Step 2: Preparation of light-colored binder
[0026] (A), feed ratio
[0027] Step 1: 25 parts by mass of the prepared polymer matrix, 75 parts by mass of petroleum resin (softening point 80° C.);
[0028] (B) According to the ratio of (A), put the ingredients into the mixing equipment, heat up to 180°C and mix, and stir for 30 minutes to obtain a light-colored cement. The main propertie...
Embodiment 2
[0030] The preparation method comprises the following steps and process conditions:
[0031] Step 1: Preparation of polymer matrix
[0032] (A) Proportion of polymer matrix
[0033] Based on 100 parts by mass of the polymer, take 100 parts by mass of styrene-butadiene-styrene triblock thermoplastic elastomer SBS, and 200 parts by mass of rubber-filled paraffin base oil;
[0034] (B) According to the ratio of (A), put each component into a high-shear force open-type rubber mixer for blending. The mixing temperature is 120°C, and the mixing time is 20 minutes.
[0035] Step 2: Production of light-colored binder
[0036] (C), feed ratio
[0037] 30 parts by mass of the polymer matrix prepared in step 1, 10 parts by mass of rubber-filled paraffin base oil, and 60 parts by mass of petroleum resin (softening point 95° C.);
[0038] According to the proportion of (A), heat each ingredient in the mixing equipment to 155°C and mix for 20 minutes to obtain a light-colored cement. Th...
Embodiment 3
[0040] The preparation method comprises the following steps and process conditions:
[0041] Step 1: Preparation of polymer matrix
[0042] (A) Proportion of polymer matrix
[0043] Based on 100 parts by mass of the polymer, take 100 parts by mass of styrene-butadiene-styrene triblock thermoplastic elastomer SBS, and 50 parts by mass of rubber-filled naphthenic and paraffin-based mixed oil;
[0044] (B) According to the ratio of (A), put each component into a high-shear force open-type rubber mixer for blending. The mixing temperature is 160°C, and the mixing time is 30 minutes.
[0045] Step 2: Preparation of light-colored binder
[0046] (D), feed ratio
[0047] 22.5 parts by mass of polymer matrix prepared in step 1
[0048] 31.5 parts by mass of rubber-filled naphthenic and paraffin-based mixed oil in any proportion, 56 parts by mass of petroleum resin (softening point 110°C);
[0049] Put all the ingredients into the mixing equipment according to the proportion of (A...
PUM
Property | Measurement | Unit |
---|---|---|
softening point | aaaaa | aaaaa |
softening point | aaaaa | aaaaa |
softening point | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com