Embodiment 1
[0049] Water-based self-adhesive decorative cloth main paint, including the following raw materials in parts by weight: 63 kg of water-based silicone modified hydroxyacrylic resin, 5 kg of SN5600 polyether modified polydimethylsiloxane additive, 0.1 kg of mixed SN9750 preservative, SN-5780 defoamer 0.3kg, 2105-3SiW substrate wetting agent 0.6kg, SN3760 non-silicon leveling agent 0.2kg, SN-7520 adhesion promoter 2.5kg, thickener 0.6kg, SN-9730pH adjustment Agent 0.3kg, SN-3896 transparent sand flour 10kg, deionized water 17.4kg, the thickener is mixed by Gel0434 thickener and Gel0620 thickener in the present embodiment, the quality of Gel0434 thickener and Gel0620 thickener The ratio is 1 / 1.
[0050] The preparation method of main paint comprises the following steps:
[0051] (1) Add half of the deionized water, preservative, defoamer, substrate wetting agent, and leveling agent into the mixing tank according to the weight component ratio, and then add water-based silicone mod...
Embodiment 2
[0056] Water-based self-adhesive decorative cloth main paint, including the following raw materials in parts by weight: 60 kg of water-based silicone-modified hydroxyacrylic resin, 5.5 kg of polyether-modified polydimethylsiloxane auxiliary agent, 0.15 kg of preservative, and defoamer 0.3kg, substrate wetting agent 0.6kg, leveling agent 0.3kg, adhesion promoter 3kg, thickener 0.7kg, pH regulator 0.4kg, transparent sand flour 9kg, deionized water 20kg, increase in the present embodiment The thickener is made by mixing Gel0434 thickener and Gel0620 thickener, and the mass ratio of Gel0434 thickener to Gel0620 thickener is 1 / 1.
[0057] The preparation method of main paint comprises the following steps:
[0058] (1) Add half of the deionized water, preservative, defoamer, substrate wetting agent, and leveling agent into the mixing tank according to the weight component ratio and mix evenly, then add water-based silicone modified hydroxyl Acrylic resin and polyether modified poly...
Embodiment 3
[0063] Water-based self-adhesive decorative cloth main paint, including the following raw materials in parts by weight: 65 kg of water-based silicone-modified hydroxyacrylic resin, 6 kg of polyether-modified polydimethylsiloxane additive, 0.2 kg of preservative, and 0.4 kg of defoamer kg, substrate wetting agent 0.7kg, leveling agent 0.4kg, adhesion promoter 4kg, thickener 0.8kg, pH regulator 0.5kg, transparent sand flour 10kg, deionized water 22kg, thickening in this embodiment The agent is made by mixing Gel0434 thickener and Gel0620 thickener, and the mass ratio of Gel0434 thickener to Gel0620 thickener is 1 / 1.
[0064] The preparation method of main paint comprises the following steps:
[0065] (1) Add half of the deionized water, preservative, defoamer, substrate wetting agent, and leveling agent into the mixing tank according to the weight component ratio and mix evenly, then add water-based silicone modified hydroxyl Acrylic resin and polyether modified polydimethylsil...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com