Sand-containing multicolor coating imitating stone-like coating and preparation method thereof
A technology of colorful paint and artificial stone, applied in the field of paint, can solve the problems of uneven effect, uneven spraying, slow construction speed, etc., and achieve the effects of low viscosity, improved stain resistance, and improved construction efficiency.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0049] A kind of sand-containing multi-color coating of artificial stone paint, in parts by mass, each component is as follows:
[0050] Granulating agent:
[0051]
[0052]
[0053] Base paint:
[0054]
[0055] Continuous phase:
[0056]
[0057]
[0058] Preparation:
[0059] (1) Prepare the granulating agent for later use: add deionized water into the container, and stir, at a stirring speed of 300-600r / min, add a dispersant, a viscosity reducer, an antifungal agent, a bactericide, a pH regulator, and stir 1-2min; adjust the stirring speed to 1300-1500r / min, add protective rubber powder and colorful anti-sedimentation agent, and stir for 50min to prepare granulator slurry;
[0060] (2) Preparation of toning base material for subsequent use:
[0061] a. Add deionized water into the container and stir;
[0062] b. Stir at 300-500r / min, add antifungal agent and dispersant evenly and slowly and stir for 1-2min;
[0063] c. Stir at 600-800r / min, add cellulo...
Embodiment 2
[0078] A kind of sand-containing multi-color coating of artificial stone paint, in parts by mass, each component is as follows:
[0079] Granulating agent:
[0080]
[0081] Base paint preparation:
[0082]
[0083]
[0084] Continuous phase:
[0085]
[0086] Preparation:
[0087] (1) Prepare the granulating agent for later use: add deionized water into the container, and stir, at a stirring speed of 300-600r / min, add a dispersant, a viscosity reducer, an antifungal agent, a bactericide, a pH regulator, and stir 1-2min; adjust the stirring speed to 1300-1500r / min, add protective rubber powder and colorful anti-sedimentation agent, and stir for 50min to prepare granulator slurry;
[0088] (2) Preparation of toning base material for subsequent use:
[0089] a. Add deionized water into the container and stir;
[0090] b. Stir at 300-500r / min, add antifungal agent and dispersant evenly and slowly and stir for 1-2min;
[0091] c. Stir at 600-800r / min, add cellulo...
Embodiment 3
[0106] A kind of sand-containing multi-color coating of artificial stone paint, in parts by mass, each component is as follows:
[0107] Granulation preparation:
[0108]
[0109] Base paint preparation:
[0110]
[0111]
[0112] Continuous phase:
[0113]
[0114] Preparation:
[0115] (1) Prepare the granulating agent for later use: add deionized water into the container, and stir, at a stirring speed of 300-600r / min, add a dispersant, a viscosity reducer, an antifungal agent, a bactericide, a pH regulator, and stir 1-2min; adjust the stirring speed to 1300-1500r / min, add protective rubber powder and colorful anti-sedimentation agent, and stir for 50min to prepare granulator slurry;
[0116] (2) Preparation of toning base material for subsequent use:
[0117] a. Add deionized water into the container and stir;
[0118]b. Stir at 300-500r / min, add antifungal agent and dispersant evenly and slowly and stir for 1-2min;
[0119] c. Stir at 600-800r / min, add ce...
PUM
Property | Measurement | Unit |
---|---|---|
glass transition temperature | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com