Antifouling antibacterial ceramic glaze and preparation method thereof
An antibacterial ceramic and antifouling technology, applied in the field of ceramic glazes, can solve the problems of ceramic surface pollution, difficulty in cleaning, affecting cleaning and aesthetics, etc., and achieve the effect of improving gloss, reducing surface energy, and preventing agglomeration
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0052] The preparation method of the antifouling and antibacterial ceramic glaze comprises the following steps:
[0053] Step 1. Weigh calcium oxide, calcium carbonate and aluminum hydroxide according to parts by weight, and mix them fully in a mixer:
[0054] Step 2: Place the phosphoric acid aqueous solution in a 55°C water bath, when the temperature rises to above 50°C, start stirring at a constant speed of 80 r / min, slowly add the uniformly mixed powder in step 1 into the phosphoric acid aqueous solution, and keep stirring at a constant speed while adding materials. ;
[0055] Step 3, after adding the material, continue to stir for 30min, then naturally cool to 25-35 ° C, put into a ball mill, add an aqueous solution of yttrium nitrate to the ball mill, and ball mill to obtain the first mixture;
[0056] Step 4. The first mixture, basic glaze slurry, antibacterial agent, dispersant and nano zinc oxide are added to the ball mill for rapid ball milling for 20min in turn, an...
Embodiment 1
[0060] The antifouling and antibacterial ceramic glaze is made from the following raw materials by weight: 50 parts of basic glaze paste, 7 parts of calcium oxide, 3 parts of calcium carbonate, 4 parts of aluminum hydroxide, 4 parts of antibacterial agent, 5 parts of nano-zinc oxide, 6 parts of 2 parts of sodium metaphosphate, 8 parts of 35% phosphoric acid aqueous solution, 2 parts of 6% yttrium nitrate aqueous solution;
[0061] The preparation method of the antifouling and antibacterial ceramic glaze comprises the following steps:
[0062] Step 1. Weigh calcium oxide, calcium carbonate and aluminum hydroxide according to parts by weight, and mix them fully in a mixer:
[0063] Step 2: Place the phosphoric acid aqueous solution in a 55°C water bath, when the temperature rises to above 50°C, start stirring at a constant speed of 80 r / min, slowly add the uniformly mixed powder in step 1 into the phosphoric acid aqueous solution, and keep stirring at a constant speed while addi...
Embodiment 2
[0068] The antifouling and antibacterial ceramic glaze is made from the following raw materials by weight: 55 parts of basic glaze slurry, 8 parts of calcium oxide, 4 parts of calcium carbonate, 5 parts of aluminum hydroxide, 4.5 parts of antibacterial agent, 6 parts of nano-zinc oxide, 6 parts of 2.5 parts of sodium metaphosphate, 9 parts of 38% phosphoric acid aqueous solution, 2.5 parts of 7% yttrium nitrate aqueous solution;
[0069] The preparation method of the antifouling and antibacterial ceramic glaze comprises the following steps:
[0070] Step 1. Weigh calcium oxide, calcium carbonate and aluminum hydroxide according to parts by weight, and mix them fully in a mixer:
[0071] Step 2: Place the phosphoric acid aqueous solution in a 55°C water bath, when the temperature rises to above 50°C, start stirring at a constant speed of 80 r / min, slowly add the uniformly mixed powder in step 1 into the phosphoric acid aqueous solution, and keep stirring at a constant speed whi...
PUM
Property | Measurement | Unit |
---|---|---|
gloss | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com