Processing method for goat hair-three-dimensional-crimped-fiber-compounded needling nonwoven carpet
A three-dimensional crimping and fiber compounding technology, which is applied in non-woven fabrics, textiles, and papermaking, can solve the problems of difficult spinning and processing, waste of goat hair resources, etc., and achieve the effect of not easy to shed hair, good elasticity, and avoiding waste
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0046] Weigh the following raw materials respectively according to mass percentage: take 75% of clean goat hair (to remove impurities and oil stains), 15% of hot-melt fiber, 15% of polyester three-dimensional crimped fiber, and the total content of the above raw materials is 100%;
[0047] Mix the clean goat hair, hot-melt fiber and polyester three-dimensional curly fiber that have been weighed to form a mixed fiber;
[0048] Adding water and crude oil-castor oil to the mixed fiber, then opening and mixing the mixed fiber successively to obtain the pretreated mixed fiber; the amount of water added is controlled to make the moisture regain of the goat hair on the machine 20%, and The total oil content after wooling is 1%; in order to make the goat hair fully absorb water and oil, it can also be subjected to veneering treatment after mixing. The veneering time is controlled at 8 hours, and the temperature is at room temperature;
[0049] Use a roller carding machine with a fiber...
Embodiment 2
[0054]Weigh the following raw materials respectively according to mass percentage: take 70% of clean goat hair (to remove impurities and oil stains), 20% of hot-melt fiber, 10% of polypropylene three-dimensional crimped fiber, and the total content of the above raw materials is 100%;
[0055] Mix the clean goat hair, hot-melt fiber and polypropylene three-dimensional crimped fiber that have been weighed to form a mixed fiber;
[0056] Add water and crude oil-castor oil to the mixed fiber, then open and mix the mixed fiber successively to obtain the pretreated mixed fiber; the amount of water added is controlled to make the moisture regain of the goat hair on the machine 22%, and The total oil content after wooling is 1.5%. In order to make the goat hair fully absorb water and oil, it can also be subjected to wool-stuffing treatment after mixing. The wool-stuffing time is controlled at 12 hours, and the temperature is at room temperature;
[0057] Use a roller carding machine w...
Embodiment 3
[0062] Weigh the following raw materials respectively according to mass percentage: take 60% of clean goat hair (to remove impurities and oil stains), 20% of hot-melt fiber, 20% of polypropylene three-dimensional crimped fiber, and the total content of the above raw materials is 100%;
[0063] Mix the clean goat hair, hot-melt fiber and polypropylene three-dimensional crimped fiber that have been weighed to form a mixed fiber;
[0064] Adding water and crude oil-spindle oil to the mixed fiber, then opening and mixing the mixed fiber successively to obtain the pretreated mixed fiber; the amount of water added is controlled to make the moisture regain of the goat hair on the machine 25%, and The total oil content after wooling is 2%; in order to make the goat hair fully absorb water and oil, it can also be subjected to wool-stuffing treatment after mixing. The time of wool-stuffing is controlled at 15 hours, and the temperature is at room temperature;
[0065] Use a roller cardi...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com