[0022] A kind of softening method of bark, comprises the following steps:
[0023] (1) Bark finishing: cut the bark on both sides of the tree, split the bark into two and peel off the tree, then cut off the bark according to the required length, which is easy to handle, reduces the bark breakage rate, and benefits The infiltration of the treatment liquid improves the treatment efficiency and obtains the bark blank;
[0024] (2) Bark alkali soaking: put the bark base in a boiled edible alkali solution with a mass concentration of 1.7%, and soak it at 80~85°C for 6 hours to promote the solution to enter the bark tissue and increase the intercellular space. Increase the pH of the bark, soften the bark fiber, take it out, and obtain the bark with alkali foam;
[0025] (3) Pickling of bark: place the bark soaked in alkali in the treatment room, spray acetic acid solution with a volume fraction of 2.3% evenly on the bark soaked in alkali, spray it repeatedly 4 times, so that the ac...
Embodiment 2
[0038] A kind of softening method of bark, comprises the following steps:
[0039] (1) Bark finishing: cut the bark on both sides of the tree, split the bark into two and peel off the tree, then cut off the bark according to the required length, which is easy to handle, reduces the bark breakage rate, and benefits The infiltration of the treatment liquid improves the treatment efficiency and obtains the bark blank;
[0040] (2) Bark alkali soaking: put the bark base in a boiled edible alkali solution with a mass concentration of 1.8%, and soak it at 80~85°C for 7 hours to promote the solution into the bark tissue and increase the intercellular space. Increase the pH of the bark, soften the bark fiber, take it out, and obtain the bark with alkali foam;
[0041] (3) Pickling of bark: place the bark soaked in alkali in the treatment room, spray acetic acid solution with a volume fraction of 2.4% evenly on the bark soaked in alkali, spray it repeatedly 4 times, so that the acetic...
Embodiment 3
[0054] A kind of softening method of bark, comprises the following steps:
[0055] (1) Bark finishing: cut the bark on both sides of the tree, split the bark into two and peel off the tree, then cut off the bark according to the required length, which is easy to handle, reduces the bark breakage rate, and benefits The infiltration of the treatment liquid improves the treatment efficiency and obtains the bark blank;
[0056] (2) Bark alkali soaking: put the bark base in a boiled edible alkali solution with a mass concentration of 1.9%, and soak it at 80~85°C for 8 hours to promote the solution into the bark tissue and increase the intercellular space. Increase the pH of the bark, soften the bark fiber, take it out, and obtain the bark with alkali foam;
[0057] (3) Pickling of the bark: Put the alkali-soaked bark in the treatment room, evenly spray the acetic acid solution with a volume fraction of 2.5% on the alkali-soaked bark, and spray it repeatedly 4 times, so that the ac...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com