[0022] A wood floor white edge color correction agent is prepared by soaking elm bark in an alkaline solution with a pH value of 9, wherein the mass ratio of the bark to the alkaline solution is 1Kg:5Kg.
[0023] The preparation method of above-mentioned wooden floor white edge repairing agent, comprises the steps:
[0024] (1) Select the elm log section that has been piled up for more than 3 months in the outdoor natural environment, directly peel off the bark on the log section, control the moisture content of the bark to 30% to 40%, and keep the shape intact, without mildew spots, Infestation, rotten bark is cut into chunks with length 70mm and width 20mm;
[0025] (2) prepare alkaline solution by ammoniacal liquor: caustic soda=10Kg: the mass ratio of 1Kg, the pH value of alkaline solution is 9, the bark of cutting short is soaked in alkaline solution for 8 hours under normal temperature, shading, sealing condition , stirring twice regularly during the soaking process, th...
Embodiment 2
[0029] A wood floor white edge color correction agent is prepared by soaking oak bark in an alkaline solution with a pH value of 10, wherein the mass ratio of the bark to the alkaline solution is 1Kg:8Kg.
[0030] The preparation method of above-mentioned wooden floor white edge repairing agent, comprises the steps:
[0031] (1) Select the oak log section that has been piled up for more than 3 months in the outdoor natural environment, directly peel off the bark on the log section, control the bark moisture content to 30% to 40%, and keep the shape intact, no mildew spots, Infestation, rotten bark is cut into blocks with a length of 100 mm and a width of 35 mm;
[0032] (2) prepare alkaline solution by ammoniacal liquor: caustic soda=9Kg: the mass ratio of 1Kg, the pH value of alkaline solution is 10, the bark that cuts is soaked in alkaline solution at normal temperature, cool and shaded, sealed condition for 6 hour, stir regularly 2 times during soaking, the mass ratio of b...
Embodiment 3
[0036] A wood floor white edge color correction agent is prepared by soaking oak bark in an alkaline solution with a pH value of 8.5, wherein the mass ratio of the bark to the alkaline solution is 1Kg: 6Kg.
[0037] The preparation method of above-mentioned wooden floor white edge repairing agent, comprises the steps:
[0038] (1) Select the oak log section that has been piled up for more than 3 months in the outdoor natural environment, directly peel off the bark on the log section, control the bark moisture content to 30% to 40%, and keep the shape intact, no mildew spots, Infestation, rotten bark is cut into blocks with a length of 100 mm and a width of 35 mm;
[0039] (2) prepare alkaline solution by ammoniacal liquor: caustic soda=12Kg: the mass ratio of 1Kg, the pH value of alkaline solution is 8.5, the bark of cutting is soaked in alkaline solution at normal temperature, cool and shaded, sealed condition for 5 Hours, regular stirring once during soaking, the mass ratio...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com