Embodiment 1
[0080] The heat exchange fins of the evaporator in the dehumidifier are made of super hydrophilic aluminum foil.
[0081] The aluminum foil includes aluminum foil and a hydrophilic layer with a thickness of 0.1 μm attached to the surface of the aluminum foil. The specific components of the hydrophilic layer are shown in Table 1:
[0082] Table 1
[0083] component
Quality Score
Cross-linked cured product of modified acrylic resin
50%
Polyol type surfactant
20%
leveling agent
29%
water
1%
[0084] Wherein, the cross-linked cured product of the modified acrylic resin is obtained by cross-linking and curing of the modified acrylic resin and trimethylol melamine as a curing agent with a mass ratio of 3:1, and the modified acrylic resin is obtained by cross-linking and curing. Bonded alkylphenol polyoxyethylene macromonomer and hydroxyl-containing acrylic prepolymer are obtained by copolymerizing for 2h at a temperature of ...
Embodiment 2
[0088] The heat exchange fins of the evaporator in the dehumidifier are prepared by using super-hydrophilic aluminum foil. The super-hydrophilic aluminum foil includes aluminum foil and a hydrophilic layer with a thickness of 0.6 μm attached to the surface of the aluminum foil. For the specific components of the hydrophilic layer, please refer to Table 2 shows:
[0089] Table 2
[0090]
[0091]
[0092] Wherein, the cross-linked cured product of the modified acrylic resin is obtained by cross-linking and curing of the modified acrylic resin and urea as a curing agent in a mass ratio of 5:1, and the modified acrylic resin is obtained by cross-linking and curing with an alkyl group having a double bond. Phenolic polyoxyethylene type macromonomer and acrylic acid prepolymer containing sulfonic acid group are obtained by copolymerization reaction for 6h at a temperature of 100°C, a pressure of 0.5MPa, and an initiator of azobisisobutyronitrile.
[0093] Among them, the alk...
Embodiment 3
[0096] The heat exchange fins of the evaporator in the dehumidifier are prepared with super-hydrophilic aluminum foil. The super-hydrophilic aluminum foil includes aluminum foil and a hydrophilic layer with a thickness of 0.3 μm attached to the surface of the aluminum foil. For the specific components of the hydrophilic layer, please refer to Table 3 shows:
[0097] table 3
[0098] component
Quality Score
Cross-linked cured product of modified acrylic resin
55%
Polyol type surfactant
10%
Leveling agents, dispersing agents and preservatives
35%
water
close to 0
[0099] Wherein, the cross-linked cured product of the modified acrylic resin is obtained by cross-linking and curing of the modified acrylic resin and glutaraldehyde as a curing agent with a mass ratio of 4:1, and the modified acrylic resin is obtained by cross-linking and curing with a double bond. Alkylphenol polyoxyethylene type macromonomer and acrylic ac...
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com