Polishing leather producing method
The technology of leather and leather embryo is applied in the field of preparation of polished leather, which can solve the problems of unsatisfactory leather polishing effect, low economic benefit of leather, limited application scope, etc. Wide range of effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] A kind of preparation method of polished leather of the present embodiment comprises the following preparation steps:
[0032] Step (1), material selection: choose the raw material of pigskin;
[0033] Step (2), cleansing treatment: spray cleansing solution on the leather embryo material, which is made by mixing ammonia water, isopropanol and ethylene glycol ether in a mass ratio of 2:1:1; cleansing solution The spraying amount is 8g / SF;
[0034] Step (3), static treatment: the skin embryo material sprayed with the cleansing water solution is left to stand at room temperature for 12 hours;
[0035] Step (4), spraying wax; spraying wax on the surface of the leather embryo after standing treatment;
[0036] Described wax agent is emulsifying wax;
[0037] Step (5), scalding: the leather embryo material after spraying the wax agent is scalded by a scalding machine;
[0038] Step (6), softening: place the scalded leather embryo material at 10°C for 24 hours, and then so...
Embodiment 2
[0040] A kind of preparation method of polished leather of the present embodiment comprises the following preparation steps:
[0041] Step (1), material selection: choose the raw material of pigskin;
[0042] Step (2), cleansing treatment: Spray the cleansing solution on the leather embryo material. The cleansing solution is made by mixing ammonia water, isopropanol and ethylene glycol ether in a mass ratio of 1.5:0.5:0.5. The cleansing solution The spraying amount is 10g / SF;
[0043] Step (3), static treatment: the skin embryo material sprayed with the cleansing water solution is left to stand at room temperature for 24 hours;
[0044] Step (4), spraying wax; spraying wax on the surface of the leather embryo after standing treatment;
[0045] The wax is polishing wax;
[0046] Step (5), scalding: the leather embryo material after spraying the wax agent is scalded by a scalding machine;
[0047] Step (6), softening: place the scalded leather embryo material at 20°C for 18 ...
Embodiment 3
[0049] A kind of preparation method of polished leather of the present embodiment comprises the following preparation steps:
[0050] Step (1), material selection: choose the raw material of pigskin;
[0051] Step (2), cleansing treatment: Spray the cleansing solution on the leather embryo material. The cleansing solution is made by mixing ammonia water, isopropanol and ethylene glycol ether in a mass ratio of 3: 1.5: 1.5. The cleansing solution The spraying amount is 12g / SF;
[0052] Step (3), static treatment: the skin embryo material sprayed with the facial cleansing solution is left to stand at room temperature for 48 hours;
[0053] Step (4), spraying wax; spraying wax on the surface of the leather embryo after standing treatment;
[0054] Described wax agent is burnt wax;
[0055] Step (5), scalding: the leather embryo material after spraying the wax agent is scalded by a scalding machine;
[0056] Step (6), softening: place the scalded leather embryo material at 30°...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com