Curved glass panel for mobile phone and forming method thereof
A technology of curved glass and curved panels, which is applied in glass forming, glass reshaping, glass production, etc. It can solve problems such as glass sticking to the mold, and achieve the effects of easy demoulding, high physical stability at high temperature, and improved stability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0048] This embodiment prepares a one-way curved 3D mobile phone glass panel:
[0049] Bending direction (X or Y direction):
[0050] Bending arc: X-direction: bending arc radius R=340mm, bending height: X-direction: height T=2.61mm, 1. Glass model: CORNING-2317 flat glass, softening temperature T=755°C.
[0051] 2. Mold preparation
[0052] Using grade: TTK-8, graphite with an average particle size of 2 μm as raw materials, to make dies and punches, the radians of the inner cavity of the dies and punches are consistent with the curved radians of the designed curved glass panel; the density of the prepared mold is 1.75 g / cm3, the Shore hardness is 75, the flexural strength is 80Mpa, the surface roughness of the concave mold and the inner cavity of the punch mold: below Ra0.08, to achieve the mirror effect;
[0053] 3. Forming of curved glass panels
[0054] Place CORNING-2318 flat glass between the graphite concave mold and the convex mold, apply a pressure of 80 g / cm2 on t...
Embodiment 2
[0062] This embodiment prepares a two-way curved 3D mobile phone glass panel:
[0063] The direction of bending (the X direction and the Y direction bend toward the Z axis at the same time);
[0064] Bending arc: X direction: bending arc radius R=140mm, Y direction: bending arc radius R=3000mm; bending height: X direction: height T=5.0mm, Y direction: T=0.5mm;
[0065] 1. Glass model: CORNING-2318 flat glass 2318, softening temperature T=768°C.
[0066] 2. Mold preparation
[0067] Using grade: TTK-8, graphite with an average particle size of 1.8 μm as raw materials, to make dies and punches, the radians of the inner cavity of the dies and punches are consistent with the curved radians of the designed curved glass panel; the prepared mold has a density of 1.80g / cm3, the Shore hardness is 80, the flexural strength is 83Mpa, the surface roughness of the concave mold and the inner cavity of the punch mold: below Ra5nm, to achieve the mirror effect;
[0068] 3. Forming of curve...
Embodiment 3
[0077] This embodiment prepares a 3D mobile phone glass panel with two sides curved:
[0078] Bending direction X: Take the distance from the outermost edge of the glass to the center of 15 as the bending centerline;
[0079] Bending arc: X direction: bending arc radius R=15mm, bending height: Z direction: height T=2.30mm,
[0080] 1. Glass model: CORNING-2320 flat glass 2320, softening temperature = 789°C.
[0081] 2. Mold preparation
[0082] Using grade: TTK-8, graphite with an average particle size of 1.9 μm as raw materials, to make a die and a punch, the radian of the cavity of the die and the punch is consistent with the curved radian of the designed curved glass panel; the density of the prepared mold is 1.78g / cm3, the Shore hardness is 78, the flexural strength is 81Mpa, the surface roughness of the concave mold and the inner cavity of the punch mold: below Ra5.0nm, to achieve the mirror effect;
[0083] 3. Forming of curved glass panels
[0084] Place CORNING-231...
PUM
Property | Measurement | Unit |
---|---|---|
height | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology