Preparation method for modified sand body
A technology for modifying sand body and production method, which is applied in the fields of sand resource utilization and desertification control, and can solve the problems of deterioration of asphalt performance, frequent sand movement, adverse effects on plants, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0100] Polyvinyl alcohol is selected as the solid organic substance that can dissolve in water;
[0101] Stir polyvinyl alcohol and water according to the weight ratio of 10:100 to form a solution;
[0102] Get 1000kg of sand, then take 155kg of solution formed by dissolving polyvinyl alcohol in water, add the solution to the sand body, then mix and stir evenly to form a modified sand body; the weight of the polyvinyl alcohol in the modified sand body and the sand body The ratio is 1:71.0;
[0103] Spread the modified sand body outdoors with a thickness of about 10cm. The water in the modified sand body is well preserved. Under the spring climate conditions in Chongqing, the evaporation is small, and the appearance of the modified sand body is similar to that of soil. For the sand body, measures such as drying are taken to make the surface dehydrated, and the surface of the modified sand body is compacted into a whole; then water is sprinkled on the surface of the modified sa...
Embodiment 2
[0107] The solid organic substance that can dissolve in water is selected from hydroxypropyl methylcellulose;
[0108] Stir hydroxypropyl methylcellulose and water according to the weight ratio of 0.35:100 to form a solution;
[0109] Take 1000kg of sand, then take 130kg of hydroxypropyl methylcellulose solution, mix the sand with the solution and stir evenly to form a modified sand body, the weight of the material hydroxypropyl methylcellulose in the modified sand body and the sand body The ratio is 1:2205;
[0110] Spread the modified sand body outdoors with a thickness of about 10cm. The water in the modified sand body is well preserved. Under the spring climate conditions in Chongqing, the evaporation is small. The grains are bonded together again, and the sand body is in a plastic wet state;
[0111] Spread the modified sand body containing grass seeds outdoors, and the water in the modified sand body is well preserved. Under the climate conditions in spring, after one ...
Embodiment 3
[0114] The solid organic matter that can dissolve in water is selected carboxymethyl cellulose sodium for use;
[0115] Stir carboxymethylcellulose sodium and water according to the weight ratio of 2:100 to form a solution;
[0116]Get 1000kg of sand, then get 187kg of sodium carboxymethyl cellulose solution, mix sand and sodium carboxymethyl cellulose solution and stir evenly to form a modified sand body, the material sodium carboxymethyl cellulose in the modified sand body and The weight ratio of the sand body is: 1:272.7;
[0117] Pave the modified sand body outdoors with a thickness of about 10cm. The water in the modified sand body is well preserved. Under the climate conditions in Chongqing in spring, the evaporation is small, and the appearance of the modified sand body is similar to that of soil. Take part of the modified sand body. body, take measures such as drying to make the surface dehydrated, and the surface plate of the modified sand body will form a whole with...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com