A technology for air purification and interior wall coatings, applied in anti-fouling/underwater coatings, polyurea/polyurethane coatings, coatings, etc., can solve the pollution of the environment by organic solution diluents, slow degradation rate of photocatalysts, failure of photocatalysts, etc. problems, to achieve good air purification ability, easy large-scale promotion, and the effect of killing bacteria and viruses
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0046] Embodiment one, this composite photocatalyst air purification water-based interior wall paint, its raw material composition is as follows by weight percentage proportioning:
[0047] Photocatalytic filler 10.5%;
[0048] Polyurethane emulsion 48%;
[0049] Propylene glycol phenyl ether 6%;
[0050] Dispersant 6%;
[0051] Stabilizer 4%;
[0052] Wetting agent 2%;
[0053] water 20%;
[0054] Antifungal agent 1.5%;
[0055] Defoamer 1%;
[0056] Leveling agent 0.5%;
[0057] Thickener 0.5%;
[0058] The photocatalytic filler is composed of nano anatase titanium dioxide and nano zinc oxide in a weight ratio of 9:1.
Embodiment 2
[0059] Embodiment two, this composite photocatalyst air purification water-based interior wall paint, its raw material composition is as follows by weight percentage proportioning:
[0060]Photocatalytic filler 15%;
[0061] Polyurethane emulsion 25%;
[0062] Propylene glycol phenyl ether 1%;
[0063] Dispersant 2%;
[0064] Stabilizer 2%;
[0065] Wetting agent 1%;
[0066] Water 45%;
[0067] Antifungal agent 4%;
[0068] Defoamer 2%;
[0069] Leveling agent 2%;
[0070] Thickener 1%;
[0071] The photocatalytic filler is composed of nano anatase titanium dioxide and nano tin dioxide in a weight ratio of 5:1.
Embodiment 3
[0072] Embodiment three, this composite photocatalyst air purification water-based interior wall paint, its raw material composition is as follows by weight percentage proportioning:
[0073] Photocatalytic filler 13.6%;
[0074] Polyurethane emulsion 41%;
[0075] Propylene glycol phenyl ether 3%;
[0076] Dispersant 4%;
[0077] Stabilizer 3%;
[0078] Wetting agent 1%;
[0079] Water 28%;
[0080] Antifungal agent 2.7%;
[0081] Defoamer 1.5%;
[0082] Leveling agent 1.4%;
[0083] Thickener 0.8%;
[0084] The photocatalytic filler is composed of nano-anatase titanium dioxide and nano-zinc oxide in a weight ratio of 1:1.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com