Modified building plastering mortar for aerated concrete
A technology for air-entrained concrete and plastering mortar, which is applied in the field of mortar production, and can solve problems such as long water absorption, hollow plastering layer, and poor bonding performance, so as to shorten the construction period, reduce procedures, and improve the economic benefits of the enterprise Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] Formula: 150kg of cement, 120kg of fly ash, 720kg of fine aggregate, 0.7kg of 40,000-viscosity hydroxypropyl methylcellulose ether, 0.4kg of polycarboxylate high-performance water reducer, 0.35kg of type II anhydrous gypsum, Redispersible latex powder 8kg, wood fiber 0.7kg, pp fiber 0.1kg, GP-SHP50 water repellent 0.9kg. Among them, the cement is ordinary Portland cement P·O 42.5.
[0018] Preparation method: first mix hydroxypropyl methylcellulose ether, high-efficiency water reducer, type II anhydrite, redispersible latex powder, wood fiber, pp fiber and water-repellent agent to obtain mixed small materials, fine aggregate When mixing , cement and fly ash, add the pre-mixed small material and mix evenly.
[0019] Example 1 Mortar performance test results are shown in Table 1.
[0020] Table 1
[0021] project
Ordinary plastering mortar
Embodiment 1 Mortar
Layered degree / mm
19
11
28-day bond strength average / MPa
0.34...
Embodiment 2
[0028] Formula: 180kg of cement, 100kg of fly ash, 710kg of fine aggregate, 0.8kg of 20,000 viscosity hydroxypropyl methylcellulose ether, 0.36kg of polycarboxylate high-performance water reducer, 0.41kg of type II anhydrous gypsum, Redispersible latex powder 10kg, wood fiber 0.6kg, pp fiber 0.08kg, GP-SHP50 water repellent 0.8kg. Among them, the cement is Portland cement P·I 42.5.
[0029] The preparation method is the same as in Example 1.
[0030] Example 2 Mortar performance test results are shown in Table 2.
[0031] Table 2
[0032] project
[0033] Detection standard is the same as embodiment 1.
Embodiment 3
[0035] Formula: 250kg of cement, 70kg of fly ash, 680kg of fine aggregate, 0.5kg of 40,000 viscosity hydroxypropyl methylcellulose ether, 0.32kg of polycarboxylate high-performance water reducer, 0.5kg of type II anhydrous gypsum, Redispersible latex powder 5kg, wood fiber 0.5kg, GP-SHP50 water repellent 0.4kg. Among them, the cement is Portland cement P·II 42.5.
[0036] The preparation method is the same as in Example 1.
[0037] Example 3 Mortar performance test results are shown in Table 3.
[0038] table 3
[0039] project
[0040] Detection standard is the same as embodiment 1.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
shrinkage | aaaaa | aaaaa |
shrinkage | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com