Method for producing bamboo-wood composite board

A production method and technology of composite boards, applied in the jointing of wooden veneers, wood processing appliances, manufacturing tools, etc., can solve problems such as large warping deformation, low static bending strength, and affecting product market development, and achieve growth cycle Short, fast-growing effect

Active Publication Date: 2012-04-04
浙江安吉双虎竹木业有限公司
View PDF8 Cites 25 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0005] However, the bamboo-wood composite boards in the prior art have problems such as large warping deformation and low static bending strength, which affect the market development of products

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Method for producing bamboo-wood composite board
  • Method for producing bamboo-wood composite board
  • Method for producing bamboo-wood composite board

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0058] Embodiment 1: a kind of bamboo-wood composite panel production method, it comprises the following steps:

[0059] (1) Preparation of core board and surface board,

[0060] ① The preparation of the core board includes the following steps in turn:

[0061] a. The air-dry density is selected as 0.45g / cm 3 Poplar, the selected wood is crushed to obtain wood particles with a particle size of 2 to 5 mm;

[0062] b. Dry the prepared wood pellets. First, put the wood pellets on a natural drying site. When the air-dried to a moisture content of 35%, send them into a drying kiln for forced drying. Control the humidity in the drying kiln to 70% for 6 days , control the temperature on the first day at 50°C, and maintain a daily heating rate of 10°C until the temperature reaches 100°C, reducing the moisture content to 9%; in order to balance the moisture content among the wood particles, it is necessary to Carry out the moisture content balance step, that is, put the dried wood p...

Embodiment 2

[0081] Embodiment 2: a kind of bamboo-wood composite board production method, it comprises the following steps:

[0082] (1) Preparation of core board and surface board,

[0083] ① The preparation of the core board includes the following steps in turn:

[0084] a. The air-dry density is selected as 0.55g / cm 3 For fir, the selected wood is pulverized to obtain wood particles with a particle size of 3 to 6 mm;

[0085] b. Dry the prepared wood pellets. First, put the wood pellets on a natural drying site. When the air-dried to a moisture content of 35%, send them into a drying kiln for forced drying. Control the humidity in the drying kiln to 80% for 5 days , control the temperature on the first day to 60°C, and maintain a daily heating rate of 10°C until the temperature reaches 100°C, reducing the moisture content to 10%; in order to balance the moisture content among the wood particles, it is necessary to Carry out the moisture content balance step, that is, put the dried w...

Embodiment 3

[0104] Embodiment 3: a kind of bamboo-wood composite board production method, it comprises the following steps:

[0105] (1) Preparation of core board and surface board,

[0106] ① The preparation of the core board includes the following steps in turn:

[0107] a. The selected air-dry density is 0.65g / cm 3 Pine wood, the selected wood is crushed to obtain wood particles with a particle size of 1 to 5mm;

[0108] b. Dry the obtained wood pellets. First, put the wood pellets on a natural drying site. When air-dried to a moisture content of 35%, send them into a drying kiln for forced drying. Control the humidity in the drying kiln to 90% for 5 days , control the temperature on the first day to 60°C, and maintain a daily heating rate of 10°C until the temperature reaches 100°C, reducing the moisture content to 11%; in order to balance the moisture content among the wood particles, it is necessary to Carry out the moisture content balance step, that is, put the dried wood parti...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
particle diameteraaaaaaaaaa
densityaaaaaaaaaa
particle diameteraaaaaaaaaa
Login to View More

Abstract

The invention relates to a method for producing a building composite rubber plate, in particular to a method for producing a bamboo-wood composite board. The method for producing the bamboo-wood composite board is implemented by the following technical scheme that the method for producing the bamboo-wood composite board comprises the following steps of: (1) preparation of a core board and a surface board; and (2) compounding process of the core board and the surface board. The bamboo-wood composite board prepared by implementing the method disclosed by the invention has the advantages of low buckling deformation and high static bending strength.

Description

technical field [0001] The invention relates to a production method of a building material composite rubber board, in particular to a production method of a bamboo-wood composite board. Background technique [0002] my country is a Shaolin country, and the per capita forest volume is less than 9.1m 3 , Timber supply and demand is very tight. In recent years, with the rise of the interior decoration industry, the demand for wooden flooring has increased sharply, but for a long time, my country's wooden floor manufacturing materials have been dependent on imports from Southeast Asia, Africa and other places. However, with the global emphasis on the ecological environment in recent years, various timber exporting countries have reduced and restricted log exports. This has caused a shortage of raw materials for wooden flooring and an increase in its price, prompting consumers to give priority to non-solid wood flooring with more reasonable prices, such as bamboo flooring, when...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): B27D1/08
Inventor 石国平
Owner 浙江安吉双虎竹木业有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products