Embodiment 1
[0014] The preparation of this example includes: based on the total weight of the catalyst, 2% NiO, 3% ZnO, 45% HZSM-5, 15% HZSM-11, 15% HMCM-22, 20% Al 2 o 3 Catalyst A.
[0015] Weigh 45 grams of HZSM-5 molecular sieve, 15 grams of HZSM-11 molecular sieve, 15 grams of HMCM-22 molecular sieve, 20 grams of Al 2 o 3 , 3.8 grams of scallop powder, mixed evenly, adding 42 grams of nitric acid aqueous solution with a mass concentration of 5%, fully kneaded and extruded into a cylindrical shape with a diameter of 1.5 mm, dried and roasted at 600 ° C for 4 hours to make 2 ~ 3 mm long catalyst support.
[0016] 20 grams of the above-mentioned catalyst carrier was immersed in 14 milliliters of zinc nitrate aqueous solution containing 0.63 grams of ZnO, left standing at room temperature for 24 hours, dried, and calcined at 450° C. for 6 hours to prepare a catalyst intermediate.
[0017] The catalyst intermediate was immersed in 14 ml of nickel nitrate aqueous solution containing 0....
Embodiment 2
[0020] The preparation of this embodiment includes: based on the total weight of the catalyst, 5% P 2 o 5 , 8% ZnO, 30% HZSM-5, 30% HZSM-11, 7% HMCM-22, 20% Al 2 o 3 Catalyst B.
[0021] Weigh 30 grams of HZSM-5 molecular sieve, 30 grams of HZSM-11 molecular sieve, 7 grams of HMCM-22 molecular sieve, 20 grams of Al 2 o 3 , 3.5 grams of scallop powder, mixed evenly, adding 42 grams of nitric acid aqueous solution with a mass concentration of 5%, fully kneaded and extruded into a cylindrical shape with a diameter of 1.5 mm, dried and roasted at 520 ° C for 4 hours to make 2 ~ 3 mm long catalyst support.
[0022] 20 grams of the above-mentioned catalyst carrier was immersed in 14 milliliters of zinc nitrate aqueous solution containing 1.84 grams of ZnO, left to stand at room temperature for 24 hours, dried, and calcined at 480 ° C for 4 hours to prepare a catalyst intermediate.
[0023] The above catalyst intermediate was impregnated in 14 ml containing 1.15 g P 2 o 5 In ...
Embodiment 3
[0026] The preparation of this example includes: based on the total weight of the catalyst, 3% NiO, 5% ZnO, 20% HZSM-5, 12% HZSM-11, 20% HMCM-22, 40% Al 2 o 3 Catalyst C.
[0027] Weigh 20 grams of HZSM-5 molecular sieve, 12 grams of HZSM-11 molecular sieve, 20 grams of HMCM-22 molecular sieve, 40 grams of Al 2 o 3 , 3.7 grams of scallop powder, mixed evenly, adding 43 grams of nitric acid aqueous solution with a mass concentration of 5%, fully kneaded and extruded into a cylindrical shape with a diameter of 1.5 mm, dried and roasted at 550 ° C for 4 hours to make 2 ~ 3 mm long catalyst support.
[0028] 20 grams of the above-mentioned catalyst carrier was immersed in 15 milliliters of zinc nitrate aqueous solution containing 1.09 grams of ZnO, left to stand at room temperature for 24 hours, dried, and calcined at 500 ° C for 4 hours to prepare a catalyst intermediate.
[0029]The catalyst intermediate was immersed in 15 ml of nickel nitrate aqueous solution containing 0.6...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com