Production method of cryolite
A production method, cryolite technology, applied in the direction of aluminum fluoride, aluminum halide, etc., can solve problems such as environmental pollution, waste of resources, and restrictions on the development of the photovoltaic industry, and achieve the goals of reducing production costs, avoiding waste, and realizing waste liquid reuse Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] The production method of cryolite of the present embodiment is raw material with the fluorine-containing waste residue of electrolytic aluminum after flotation and the by-product of producing polysilicon material, comprising the following steps:
[0016] (1) Weigh 100g of electrolytic aluminum fluorine-containing waste slag after flotation and 60g of monocryolite by-product of polysilicon production;
[0017] (2) Mix the fluorine-containing waste residue of electrolytic aluminum after flotation in step (1), monocryolite by-product of polysilicon material production, and 1500g of fluorine-containing hydrochloric acid solution, and then stir and react at 90°C for 1 hour, then Filtrate, wash the filter cake with water, and dry the filter cake to obtain a cryolite product. The content of fluorine in the cryolite product is 52% by weight. The obtained filtrate and washing liquid are treated with lime and discharged.
[0018] Wherein the weight percentage content of Al in the...
Embodiment 2
[0020] The production method of cryolite of the present embodiment is raw material with the fluorine-containing waste residue of electrolytic aluminum after flotation and the by-product of producing polysilicon material, comprising the following steps:
[0021] (1) Weigh 100g of electrolytic aluminum fluorine-containing waste slag after flotation and 100g of monocryolite by-product of polysilicon production;
[0022] (2) Mix the fluorine-containing waste residue of electrolytic aluminum after flotation in step (1), the monocryolite by-product of polysilicon material production, and 200g of fluorine-containing hydrochloric acid solution, and then stir and react at 20°C for 6 hours, then Filtrate, wash the filter cake with water, and dry the filter cake to obtain a cryolite product. The content of fluorine in the cryolite product is 53.2% by weight. The obtained filtrate and washing liquid are treated with lime and used to produce calcium chloride.
[0023] Wherein the weight pe...
Embodiment 3
[0025] The production method of cryolite of the present embodiment is raw material with the fluorine-containing waste residue of electrolytic aluminum after flotation and the by-product of producing polysilicon material, comprising the following steps:
[0026] (1) Weigh 100g of electrolytic aluminum fluorine-containing waste slag after flotation and 50g of monocryolite by-product of polysilicon production;
[0027] (2) Mix the fluorine-containing waste residue of electrolytic aluminum after flotation in step (1), the monocryolite by-product of polysilicon material production, and 2250g of fluorine-containing hydrochloric acid solution, and then stir and react at 50°C for 2 hours, then Filtrate, wash the filter cake with water, and dry the filter cake to obtain a cryolite product. The content of fluorine in the cryolite product is 55% by weight. The obtained filtrate and washing liquid are treated with lime and used to produce calcium chloride.
[0028] Wherein the weight perc...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com